06.10.2014 Views

Handbook for Bridge Inspections - TSP2

Handbook for Bridge Inspections - TSP2

Handbook for Bridge Inspections - TSP2

SHOW MORE
SHOW LESS

You also want an ePaper? Increase the reach of your titles

YUMPU automatically turns print PDFs into web optimized ePapers that Google loves.

Norwegian Public Roads<br />

Administration<br />

• •<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong><br />

<strong>Inspections</strong><br />

D es embf>,2005


Norwegian Public Roads<br />

Administration<br />

<strong>Handbook</strong> <strong>for</strong><br />

<strong>Bridge</strong> <strong>Inspections</strong><br />

Desember 2005


Copyright<br />

Copyright © 2000-01-1 2 by Norwegian Public Roads Administration.<br />

A ll ri ghts reserved under the International Copyright Conventions. This book is part of the<br />

Norwegian <strong>Bridge</strong> Management System, developed and owned by the Publ ic Roads<br />

Admini strati on in Norway. and may not be reproduced in w hole or in part in any foml or by<br />

any means, electronic or mechani cal, including photocopyi ng, recording or by any<br />

infommtion storage and retrieval system now known or hcreancr invented, without tbe prior<br />

written permission of the Copyright holder.<br />

Exception:<br />

Any Customer of the Norwegian <strong>Bridge</strong> Management System is an authorised Copydght<br />

holder <strong>for</strong> thi s handbook with in their jurisdiction. This authorisation may be extcndcd by the<br />

Customer to any person or company within the borders of the nali ve country <strong>for</strong> a particular<br />

assignment. The Customer is also authorised to ut il ise thi s <strong>Handbook</strong> when they are involved<br />

in international assignments.


INTRODUCTION<br />

<strong>Bridge</strong> inspections are essential with regards to safeguard the bridges and keep properly management<br />

of the bridge assets. Assessment of risk and prediction of future conditions are all elements<br />

which a <strong>Bridge</strong> Management System has to deal with. The examination of the present c ondition and<br />

o f expected deterioration leads to the detenninati on o f strategies <strong>for</strong> the interventions. T he process<br />

is completed by the execution and control of the repairs. It is there<strong>for</strong>e obvious that consistent<br />

inspections of bridges are important , not only <strong>for</strong> the bridge safety as such, but also in order to keep<br />

the infrastructure sufficiently operating <strong>for</strong> the society.<br />

Hence that the Norwegian BMS is developed to facilitate all aspects of bridge maintenance and<br />

management, it contains additionally to the handbooks al so an advanced computerised system<br />

avai lable <strong>for</strong> handling both the required inventory, inspection and maintenance data. A complete,<br />

user-fri endl y, accurate, and compatible database constitutes the foundat ion of our bridg e management<br />

system.<br />

This Inspection <strong>Handbook</strong> has been prepared to coverthe requirements of the staffinv()lved in<br />

<strong>Bridge</strong> <strong>Inspections</strong>, and it provides thorough and detailed guidance on Damage Evalua ti on.<br />

Emphasis has been made 10 explaining a wide range of different types of damage on different Iy pes<br />

of structures by means of photos in connection with explanatory damage Evaluati on guiding. The<br />

photos have been used ex tensively to facilitate a better understanding as "seeing is beli eving".<br />

In the BMS, all data is intended to be stored in computers. To avoid mistakes and to make the<br />

System consistent with regard to th e computeri sation, a numerical code <strong>for</strong> di ffe rent typ es of damage<br />

and cause of damage have been introduced. These are presented in chapter 5 and irl the<br />

Appendi ces of the <strong>Handbook</strong><br />

References are made to different handbooks from the Norwegian Public Roads Admiinistration.<br />

These have 10 be altered with simular handbooks issued at the National Road Authori1y.


Foreword<br />

<strong>Inspections</strong> of hridges are among the main objectives which every<br />

Road Manager has to take serious in order to ful fi l its obligations<br />

to achi eve a safe and secure management, operation aJ1d maintenance<br />

orlhe country's bridges. Superior obligations atld requireme<br />

nts <strong>for</strong> the inspection of bridges arc stated in the "Guideli nes<br />

<strong>for</strong> the Management of <strong>Bridge</strong>s".<br />

This <strong>Handbook</strong> deals with all types of routine and per iodie inspections<br />

to be carried out on all bridges. <strong>Bridge</strong> inspcctio:n is defined<br />

as: "Visual checks of bridges combined with measurem ents and<br />

materials investi gations in order 10 determine the condition and<br />

safety level ofhridges. The <strong>Inspections</strong> shall identi fy 1he needs <strong>for</strong><br />

remedial actions, any req uired maintenance or repair activities in<br />

general and the strengthening or rebuilding of any bri c:ige within<br />

the jurisdiction o f the Road Manager".<br />

The purpose of the <strong>Handbook</strong> is to offer guidance on bridge<br />

inspections in order to provide a sustainable and unified system <strong>for</strong><br />

bridge inspectors th roughout the entire country.<br />

It is envisaged that every modem <strong>Bridge</strong> Managemen t System<br />

should have a databased computer system, handling both inventory,<br />

inspection and maintenance data. The foundation <strong>for</strong> detennining<br />

the repairs and maintenance activities on bridges w il l be the<br />

results oflhe bridge inspection data recorded in Brutu s<br />

International which also constitute the basis <strong>for</strong> the budget<br />

requirements when composing the budget. The BMS system provides<br />

recommendations <strong>for</strong> structura l maintenance an.d strategy.<br />

<strong>Bridge</strong> Inspectors are exposed to many ri sks during in spections,<br />

e.g. being struck by vehicles, fa lling from the super or. substructure<br />

etc .. Safety equipment, safety precautions and safety requirements<br />

are there<strong>for</strong>e important aspects to be included both in this<br />

<strong>Handbook</strong> and during the inspection procedures.<br />

The Inspection <strong>Handbook</strong> is developed by NPRA 's <strong>Bridge</strong><br />

Departme nt.<br />

This edition have been sl ightl y corrected compare to t he<br />

previous edition of February 200 I.<br />

The Directorate of Publ ic Roads,<br />

Desember 2005


TA BLE OF CONTENTS<br />

Introductiont<br />

Acknowledgements<br />

Foreword<br />

3<br />

4<br />

5<br />

I Inspection of <strong>Bridge</strong>s<br />

1.1 General<br />

1.2 Inspection Types<br />

2 Terminology<br />

2.1 Location System<br />

2. 1.1 General<br />

2. 1.2 The Consept of Division by Axis<br />

2.1.3 The Division by Axes <strong>for</strong> Big <strong>Bridge</strong>s<br />

2. 1.4 Location System when Beams<br />

2. 1.5 Reflected Plan of the Superstructure<br />

2. 1.6 Reflected Plan of Columns and Foundat ions<br />

3 Planning of Inspection<br />

3. 1 General<br />

3.2 Inspecti on Plan<br />

3.3 Inspection Programme<br />

3.4 Inspection Fonns<br />

3.5 Inspection Resources and Safety Precautions<br />

3.5. 1 General Req ui rements of the Inspectors<br />

3.5.2 Inspection Tools<br />

3.5.3 Safety Precautions<br />

4 Inspection Tools and Access Equipment<br />

4.1 Inspecti on tools<br />

4. 1.1 Personal/protective equipment<br />

4. 1.2 Ordinary Inspection Tools<br />

4.1.3 Inspection Tools <strong>for</strong> general inspection<br />

4. 1.4 Inspection Tools <strong>for</strong> Major Inspection<br />

4. 1.5 Inspection Tools <strong>for</strong> Special Inspection<br />

4. 1.6 Inspection Tools fo r Major Underwater-Inspec;tion<br />

4. 1.7 Inspection Tools <strong>for</strong> Major Cable-Inspection<br />

4.2 Access Equipment<br />

4.2. 1 General Inspection<br />

4.2.2 Other <strong>Inspections</strong><br />

4.2.3 Ladder<br />

4.2.4 Ordinal)' type of Lifts<br />

4.2.5 Types of <strong>Bridge</strong> Lifts<br />

4.2.6 Other types of Access Eq ui pment<br />

5 Damage Evaluation Fundamentals<br />

5.1 General<br />

5.2 Types of Damage<br />

5.3 Degree of Damage - Consequence of Damage<br />

5.3. 1 Degree of Damage<br />

12<br />

15<br />

21<br />

25<br />

41<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong><br />

7


5.4 Damage Eva luation<br />

5.4.1 Primary & Secondary Damage<br />

5.4.2 The Extent to which Damage has Developed<br />

5.4.3 Compound (Combined?) Damage<br />

5.5 Prioriti sing Maintenance<br />

5.6 Ca use(s) of Damage<br />

6 Carrying out In spections 59<br />

6. 1 Acceptance Inspection<br />

6. 1. 1 Scope 50<br />

6. 1.2 Visual Checking<br />

6.2 Warranty Inspection<br />

6.2.1 Scope<br />

6.2.2 Visual Checking<br />

6.3 Gcncral lnspecli on<br />

6.3.1 Scope<br />

6.3.2 Basic General lnspeclion<br />

6.4 Major inspection<br />

6.4.1 Scope<br />

6.4.2 Visual Inspection<br />

6.5 Major Inspection of Cables<br />

6.5.1 Objective and Scope<br />

6.5.2 V isual <strong>Inspections</strong><br />

6.6 Major Inspection · Underwater<br />

6.6.1 Scope<br />

6.6.2 Visual <strong>Inspections</strong><br />

6.7 Special Inspection<br />

6.7. 1 Scope of inspection<br />

6.7.2 Visual Checking<br />

6.8 Ma intenance Measures - Extent of Damage<br />

7 Surveys, Materials Tests and Instrumentation 83<br />

7. 1 General<br />

7.2 Surveys (Type of measurements)<br />

7.2.1 Levell ing<br />

7.2.2 Horizontal Distances/Disp lacement<br />

7.2.3 Measuring the Thickness of Wearing Surfaces<br />

7.2.4 Measuring of Ruts<br />

7.2.5 Measuring Evenness orthe Deck Surface<br />

7.2.6 Measuring Sag<br />

7.2.7 Recording <strong>Bridge</strong> Details<br />

7.2.8 Measuring ofVcrt ical Clearance<br />

7.3 Adequate Materials In vestigation - Concrete<br />

7.3.1 Locating the rcin <strong>for</strong>cemcn t - Measuring its Cover<br />

7.3.2 Measuring the Depth of Carbonation<br />

7.3.3 Measuring Chloride Content<br />

7.3.4 Corrosion Testing (EC P)<br />

7.3 .5 Detennining the Level of Strength<br />

7.3.6 Structural Analysis<br />

7.3.7 Inspecti on of Prestressed Tendons<br />

7.3.8 Cutting open the Concrete to Assess the Corrosion level<br />

7.3.9 Location of Materials Testing <strong>for</strong> Concrete Coastal <strong>Bridge</strong>s<br />

8 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


7.4 Adequate Materials Testing - Steel<br />

7.4. 1 Checking the Torque of Screws<br />

7.4.2 Checking Rivets and Scrcws<br />

7.4.3 Checking Welds<br />

7.4.4 X-ray Check<br />

7.4.5 Ultrasound Check<br />

7.4.6 Magnetic Powder Check<br />

7.4.7 Fibre Optics<br />

7.4.8 Ultrasound Measurement of Material Thickness<br />

7.5 Adequate Materia ls In vestigal'ions - Timber<br />

7.5. 1 Invcstigation o f the humid ity levcl of Timber<br />

7.5.2 Checking fo r Fungus and ROI- Timber<br />

7.6 Adequate Material s Investi gation - Stone<br />

7.6. 1 Compressive Strength <strong>for</strong> Stone<br />

7.7 Adequate chccking ofthc Surface Trcatment<br />

7.7. 1 Thickness of Surface Coating - Concrete<br />

7.7.2 Adhesive bonding between Surface Coating a:nd Concrete<br />

7.7.3 Depth of Penetration of Water Repellent Improegnation<br />

7.7.4 Thickness of Surface Coaling of Steel<br />

7.7.5 Adhesive Bonding bctwecn Surface Coaling


9.3.8<br />

9.3.9<br />

9.3. 10<br />

9.3. 11<br />

9.4 Stone and Masonry Elements 227<br />

9.4. 1<br />

9.4.2<br />

9.4.3<br />

9.4.4<br />

9.4.5<br />

9.4.6<br />

9.4.7<br />

9.5 Timber Elements 24 1<br />

9.5.1<br />

9.5.2<br />

9.5.3<br />

9.5.4<br />

9.6 Wearing Courses & Waterproofin g Layers 259<br />

9.6.1<br />

9.6.2<br />

9.6.3<br />

9.6.4<br />

9.6.5<br />

9.6.6<br />

9.6.7<br />

9.6.8<br />

9.6.9<br />

9.6. 10<br />

9.7 Bearings & Bcaring Scats/Shelves 289<br />

9.7. 1<br />

9.7.2<br />

9.7.3<br />

9.7.4<br />

9.7.5<br />

9.7.6<br />

9.7.7<br />

9.8 Joints & Thresholds 297<br />

9.8.1<br />

9.8.2<br />

9.8.3<br />

9.8.4<br />

9.8.5<br />

9.8.6<br />

9.9 Parapets 305<br />

9.9.1<br />

9.9.2<br />

9.9.3<br />

9. 10 Water Drainage System 32 1<br />

9. 10.1<br />

9. 10.2<br />

10 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9. 10.3<br />

9.10.4<br />

9.11 Other Equipment & Attached Utilities<br />

9. 11.2<br />

9. 11.3<br />

9.12 Codes<br />

327<br />

333<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong><br />

11


1. Inspection of<br />

<strong>Bridge</strong>s<br />

Guidel ines<br />

1.1 General<br />

Reference is made to "Guidelines <strong>for</strong> the Management of <strong>Bridge</strong>s"<br />

as superior guidance on management of bridges. To fu lfi I their<br />

obligations with regards to bridge management, the compUlerised<br />

Brutus International <strong>Bridge</strong> Management Syst.em (BMS) is<br />

intended to be the assisting tool <strong>for</strong> conducting the duties stated in<br />

the Guidelines.<br />

The planning of inspections, entering the results from pc rfonned<br />

inspections into the computerised part as well as composing and<br />

recommending all relevant remedial actions to be taken on<br />

bridges, sha ll be done by using the Brutus International.<br />

1.2 Inspection Types<br />

The inspection types re flect the thoroughness and frequency of<br />

inspections.<br />

The first In spectio ns<br />

The bridge inspection cycle starts when construction is completed<br />

at which point the fo llowing inspection types shall be pe:r<strong>for</strong>med:<br />

* Acceptance Inspection<br />

'" Warranty Inspection<br />

Ro ut ine Inspectio ns<br />

After the bridges have been handed over, routine inspect ions shall<br />

be carried out <strong>for</strong> the remaining bridge's service life time. This<br />

involves the following in spection types:<br />

'" General Inspection<br />

'" Major In spection<br />

'" Major Inspection of Cabl es<br />

'" Major Underwater lnspection<br />

Additio na l <strong>Inspections</strong><br />

General inspection intend to be carried out also during the warran·<br />

ty (guarantee) period.<br />

To complement the above mentioned inspections, or in tbe event<br />

of extraordinary occurrences there may be a need to perfonn:<br />

'" Special Inspection<br />

Purpose of Inspectio ns<br />

In the following, descriptions of purposes of the inspecti ons are<br />

outl ined. For more det"ailed descriptions, reference is ma de to<br />

Chapter 6 of this <strong>Handbook</strong> or to the "Guidel ines <strong>for</strong> the<br />

Management of Bri dges".


Acceptance Inspection<br />

Warranty Inspection<br />

General Inspection<br />

Major Inspection<br />

Major Inspection Cables<br />

Major Inspection<br />

Underwater<br />

Special Inspection<br />

The Acceptance Inspection is the first type of inspection to be carried<br />

out after the completion of a new bridge. The purpos e is to<br />

accept or not the acceptance criteria fo r the take-over res.ponsibility<br />

of the bridge owner, where the acceptance criteria is to uncover<br />

any deficiencies, damage or defects to the structure which have<br />

arisen during the construction phase, as well as identifyillg inappropriate<br />

design sol utions and any sources of deterioratio n that<br />

may be of significance in conjunction with future maintenance.<br />

Acceptance Inspecti on shall also be per<strong>for</strong>med after maj~ r rehabilitat<br />

ion or maintenance works have been carried out on a "bridge.<br />

The purpose of the Warranty Inspecti on is to chec k that a ny work<br />

done during the construct ion phase, or repairs following<br />

theAcceptance Inspection are acceptable, and that new damage,<br />

faults or de ficiencies have not occurred to the bridge.<br />

Any new sources of deterioration of relevance <strong>for</strong> later maintenance<br />

should also be identifi ed.<br />

The purpose of the General Inspection is to check if any serious<br />

damage affecting the load canying capacity, traffic safety, fu ture<br />

maintenance or environment/aesthetic have appeared to lhe structu<br />

re<br />

The purpose of Major Inspection is 10 ensure that the ent ire bridge<br />

is funct ional, detenn ining any needs <strong>for</strong> maintena nce actions<br />

including making cost estimates <strong>for</strong> these. The inspectioll includes<br />

also taking measurements and materials investi gations iEnecessary.<br />

The purpose of Major Inspection of Cables is to evaluate any damage<br />

to cables, hangers inclusive clamps and anchorage plOi nts to<br />

verify their funct ionali ty. Remedial actions incl usive cos.t estimates<br />

shall also be dctennined.<br />

The purpose of Major Underwater In spection is to check. the condition<br />

of any bridge elements unden.vater to ensure their fu nctionality.<br />

The river bed in the vicinity of the bridge shoul d also be<br />

checked. Remedial actions inclusive cost estimates shall be determined.<br />

The purpose of Special Inspection is to investigate close .. any damage<br />

and the cause of damage observed during previous inspections,<br />

but also to fonn the basis <strong>for</strong> any description of costly and/or<br />

complicated action wh ich might be recommended.<br />

Special inspections are not being carried out at regular intervals,<br />

but can be triggered off from the fo llowing:<br />

'" Requ irements from previous major inspections<br />

'" Accidents such as impact damage from vehicles<br />

'" Overloading<br />

'" Flood or flooding<br />

'" When experience from similar types of bridges and en-.i ronment<br />

so indicates


2 TERMINOLOGY<br />

Location System<br />

2.1 The location System<br />

2.1 .1 General<br />

It is important that everybody uses the same way to describe where<br />

a damage is located on a bridge and where measurem ents and<br />

material in vestigations are carried out. There<strong>for</strong>e, on all bridges, a<br />

localisation system shall be established to make this possible.<br />

The following sections illustrate how such a system can be<br />

planned by using axi s, the numbering of beams and the projection<br />

of columns, superstructure etc ..<br />

In case such a system has been prcviously establi shed <strong>for</strong> the<br />

bridge, thi s shall be continued or integrated in the new system.<br />

Divisio n by Axes<br />

2.1.2 The Concept of Division by Axes<br />

All bridges sha ll be di vided into an axis number by each abutment<br />

and each column. The div ision by axcs shall be recorded in BRU­<br />

TUS and thereby appear on the inspection fonns.<br />

The main rule is that the di vision being used on the construction<br />

draw ings or as built drawings shall be used.<br />

Numbering the<br />

Axes<br />

Ifno system with regard to axes has been used on the drawings,<br />

axis I (or axis 0) shall be placed at the abutment with the lowest<br />

kilometre in relation to the kilometre direction on the road. On the<br />

draw ings of the bridge, axis I shall be to the left. As a. reference,<br />

designations like column axis 2, superstructure ax.is 2-3 etc. shall<br />

be used.<br />

At the abutments the geographical di rection or the closest village<br />

sha ll be used to detennine the direction of a xes geographical. The<br />

division by axes can with advantage be marked with s pray on larger<br />

bridges. However, this must be done with care to a"Void a spoil-<br />

Figllre 2.1-1: Exumple o/Numbering rhe Axes<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 15


2.1.3 The Division by Axes <strong>for</strong> Big <strong>Bridge</strong>s<br />

For arch bridges, truss bridges, suspension bridges an


Hangers<br />

/ ® ®<br />

23456189<br />

Suspension <strong>Bridge</strong>s<br />

Figllre 2. 1-4: .'Vllmbering 'he AxeslHangers on Suspension Br idges<br />

Bundle of Cables<br />

Left hand-side<br />

6 5 432<br />

~ :<br />

Layers<br />

:mm<br />

Right tland-side<br />

123456<br />

Figllre 2. 1-5: .'VlIIl1bering 'he Cable Bundles 011 S1Ispellsioll liridges<br />

@ ®<br />

®<br />

Cable Stayed <strong>Bridge</strong>s<br />

2345678<br />

Connection ints<br />

Figure 2./-6: Dirisioll of Axis 0 11 Cable Stayed <strong>Bridge</strong>s<br />

Cross Sections<br />

2.1.4 Location System when Beams<br />

All cross sections shall be sketched looking in the direction of the<br />

chainage (nonna1l y identical to the direction of inc reasing axisnumbering).<br />

Designation of where the cross sectioll is taken can<br />

<strong>for</strong> example be axis 3 + 5 m, see Figure 2. 1-7.<br />

Left hand-side or right hand-side can be used to assign precise<br />

localisation of details of a cross section. Alternative ly,<br />

upstream/downstream or geographical directions c an be used.<br />

Cross secti ons of beams shall be assigned using letters, alternati<br />

vely numbers, marked from left to right.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 17


Numbering of Beams<br />

1 r<br />

~·~~'.~I VII! ~~> .. - ...<br />

Cross-section 01 Axis 3+5<br />

Figllre 2./-7: Cross Seclioll 0/(/ Be(/III <strong>Bridge</strong><br />

Reflected Plan of<br />

Superstructure<br />

2.1.5 Reflected Plan of the Superstructure<br />

In some cases it can be rel evant to make a reflected pl.an of the soffit<br />

of the superstructure in order to locate the defects and testing<br />

spots Exampl e of a refl ected plan of a beam bridge is shown in<br />

Figure 2. 1-8 and Figure 2. 1-9.<br />

- 1<br />

-<br />

2<br />

'V<br />

/'.<br />

Figllre 2./-8: Exampleo/Foldillg 0111 o/u Beam <strong>Bridge</strong><br />

18<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


Figure 2. 1-9: Example of a Reflecled Plan of a Box Girder BiI·illge<br />

2.1 .6 Reflected Plan of Columns and<br />

Foundations<br />

For rectangu lar columns, surface I shall be facing the lowest axis<br />

number. The remaining surfaces shall be numbered against the<br />

clockwise direction. The re flected plan shall make it possible to<br />

look at each surface in such a way that sides with jo intly comers<br />

are naturally tied together. The column is folded alii al the corner<br />

between surface 1 and 4 in a clockwise direction. S ee Figure 2. 1-<br />

10.<br />

-k. +100<br />

....c<br />

.<br />

,~ D.15M<br />

- ..<br />

..-<br />

,~<br />

•<br />

Reflect ed Pla n of a<br />

Rectangular Co lumn<br />

K=altitude<br />

Flate=surface<br />

k. +2,<br />

....c<br />

9<br />

•<br />

2<br />

Surface 3<br />

3 4<br />

Surface 4<br />

Surface 1<br />

Surface 2<br />

Fig. 2. /-10 Numbering of surfaces ami the folding 01/1 of a re c/allglliar colllllln<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 19


Circular columns are di vided according to the watch as shown in<br />

figure 2. 1- 11. The folding takes place by opening the column at<br />

12 o'clock and then fold to both sides. The folded col umn starts<br />

with the 12 o'clock spot at the left hand-side of the plan and fin ishes<br />

with 00 o'clock to the right.<br />

Reflected Plan of a<br />

Circular Column<br />

~ + 10,0<br />

,---~--~----~--,<br />

k. +2,C<br />

,---<br />

~-- c-----~------~----~o_----~<br />

12 09 06 03 00<br />

•<br />

06<br />

Figure 2.1-11: £.ml/lple 0/ Rejleclel/ Plan O/ll Circular ColwlII~<br />

20<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong>


3 Planning of<br />

Inspection<br />

Planning Procedures <strong>for</strong><br />

the <strong>Inspections</strong><br />

3.1 General<br />

Planning of inspections includes all relevant tasks from detennination<br />

of which bridges shall be inspected to the per<strong>for</strong>mance of the<br />

inspection. It is assumed that most of tile duties shall be carri ed out<br />

by assistance from the computerised part of the BMS.<br />

The planning phase includes the foll owing:<br />

• Make inspection plans<br />

'" Make inspection programme<br />

* Pri nt out inspecti on fonns<br />

'"<br />

'"<br />

'"<br />

Determine necessary inspection too ls<br />

Determine necessary access equipment<br />

Pl an and prepare necessary man <strong>for</strong>ce, waming signs, safety<br />

requirements etc.<br />

Examples of inspection tools and access equipment are more thoroughl<br />

y ex plained in chaptcr4. The other items li sted above are<br />

further elaborated in this chapler.<br />

Reference should also be made to chapter 6 "Carrying Out<br />

<strong>Inspections</strong>" and chapter 7 "Surveys, Materials Tests and<br />

Instru mentation".<br />

For major underwater inspections, it is recommended to carry out<br />

the inspections during the most appropriate season, that means<br />

when the water level is low, the water speed is slow and the sight<br />

in the water is good.<br />

Inspection plan<br />

3.2 Inspection Plan<br />

All bridges shall have an inspection pl an in the computerised part<br />

of the BMS, where the fo llowing shall be included:<br />

* Decide whi ch inspections shall be carried out<br />

>I< Detennine and sc hedule the di fferent inspections (programme);<br />

that means detcrmination of date, year and frequencics<br />

>I< Elements to be inspected fo r the different inspection types<br />

>I< Measurements, material investigations and read ing off instru<br />

mentation planned <strong>for</strong> on eaeh ind ividual inspection, inclusive<br />

extent of the work and exact time schedule<br />

>I< Determination of special damage/elements that need special<br />

attention<br />

>I< Determine required access equipment <strong>for</strong> the different inspec<br />

tions


When New <strong>Bridge</strong>s<br />

Ex isting <strong>Bridge</strong>s<br />

Inspection Programme<br />

Sub Programmes<br />

When new bridges, Ihe inspection plan is equal to the Acceptance<br />

Inspection. Practical experience shows however, that in most<br />

cases, the inspection plan is being carried out after th~ handingower<br />

process, and then based on the report from the acceptance<br />

inspection .. However, the Acceptance Inspection shall nevertheless<br />

be planned fo r in the inspection plan and the results recorded.<br />

For existing bridges, the Major Inspection shall be the: basis <strong>for</strong><br />

establishing the inspection plan if the latter do not ex ist. In the<br />

case where the inspection plan is unsatisfactory fi lled in, the data<br />

from the Major Inspection can be used as supplement or as amendment.<br />

3.3 Inspection Programme<br />

An inspection programme is a listing of all bridges decided <strong>for</strong><br />

inspection in a specific yea r. The Inspection Programme contains<br />

also measurements, material investigations, levell ing ~tc. that shall<br />

be carried out during the schedul ed inspections <strong>for</strong> each bridge.<br />

The in spection programme shall provide an overview to the<br />

<strong>Bridge</strong> Engineer and his superiors on whi ch bridges ar e to be<br />

inspected in a current year.<br />

The Inspection Programme can be split into sub-inspe::clion programmes<br />

grouped by different inspection types, road number,<br />

bridge types, districts etc._The status of bridge inspec1ion <strong>for</strong> each<br />

bridge is visualised in the programme by means of di fferent background<br />

- colours in the column <strong>for</strong> the current inspecti...on year like:<br />

White: You are free to fi ll in the inspection type and. year you<br />

wanl.<br />

Orange: The bridge is currently under inspection, me aning that<br />

the inspection <strong>for</strong>m has been printed out <strong>for</strong> the bridge.<br />

Green: The inspection has been completed as planned and data<br />

entered.<br />

Red: The inspection date has expired and you are behind<br />

schedule. (No data entered)<br />

Inspection Forms<br />

3.4 Inspection Forms<br />

Based on the decisions made in the inspection programme <strong>for</strong> the<br />

bridges in question, the programme prints out individual inspection<br />

fonns <strong>for</strong> each bridge fo r the selected inspection type.<br />

When printing out inspection <strong>for</strong>ms <strong>for</strong> each bridge, there is a possibility<br />

of selection of transferring previous inspection data to be<br />

included in the present inspection <strong>for</strong>m or not.


3.5 Inspection Resources and<br />

Safety Precautions<br />

3.5.1 General Requirements of the Inspectors<br />

In order to have reliable inspection data, it is very important thai<br />

the data entered into the system is as correct as possibl e.<br />

Inspection data is fundamentally based on judgements made by<br />

the inspectors, and their quality depends very much on the skill s<br />

and bridge experience they have gained. There<strong>for</strong>e, it is important<br />

that the inspeclors have specific quali fications such as accuracy<br />

and reliabili ty, and arc properly trained in BMS.ln additi on, an<br />

inspector has to be a careful worker, and he/she must be in good<br />

health and responsibl e (docs nol take unnecessary risks).<br />

Be<strong>for</strong>e the inspection starts, it is very important that the inspector<br />

clarifies tbe obligati ons and responsibi lities of the staff in volved in<br />

the in spection process. Each person in volved in the inspecti on<br />

must know what hi s or hers duties are. It is the inspector's responsibility<br />

to provide all personnel involved in the inspection with relevant<br />

inspection tools and safety equipme nt.<br />

Tra ining<br />

However, it is the <strong>Bridge</strong> Engineer's responsibility to train and<br />

equip the inspection personnel properl y within all aspects of<br />

inspection procedures and safety routines and to provide adequate<br />

tools and equi pment to the inspectors. Generally speaking, the<br />

<strong>Bridge</strong> Engineer should be responsible <strong>for</strong> all aspects within the<br />

fi elds of securing Health, Environment and Safety at the inspection<br />

site.<br />

3.5.2 Inspection Tools<br />

In order to per<strong>for</strong>m Ihe different types of inspections, different<br />

lools and equipment have to be used. These include non-sophisticated<br />

tools which wi ll be termed ordinal)' and spec ialised tools <strong>for</strong><br />

specific unique jobs which will be used depending on the type of<br />

inspection and site conditions. There are nonnally no inspecti on<br />

lools and equipmenl <strong>for</strong> an infonnal inspection but <strong>for</strong> the other<br />

types of inspections, the lools and equipment li sled in chapter 3<br />

should be made availabl e:<br />

3.5.3 Safety Precautions<br />

The safety of bridge inspectors and road users during the inspection<br />

fall s within the responsibility of the <strong>Bridge</strong> Engineer. It is<br />

important that he/she ensures that they frequent ly get appropriate<br />

training in safety procedures and especially w hen new inspectors<br />

have been employed.<br />

Possibilities of injury arise mainl y from:<br />

* Traffic on the deck or approaches.<br />

* A fall from the superstructure to the river or road below.


• Attack from insects, repti les, animals or vegetation around the<br />

bridge.<br />

To try to alleviate these dangers, there should be at least two people<br />

when per<strong>for</strong>ming an inspection. One might be the driver, who<br />

can also assist when tak ing measurements.<br />

Always use the safety eq ui pment fo r yourself and on the road,<br />

even on roads with very light traffic. When inspecting bridges<br />

crossing rivers with high speed currents it is important to use a<br />

li fe-jacket and safety-rope.<br />

It is always important to remember tha t accidents occur without<br />

warmng.


4. Inspection Tools &<br />

Access Equipment<br />

When inspecting bridges the inspector always has to bring with<br />

him different kinds of equipment. The necessary equipment<br />

depends on the type of bridge to be inspected and the type of<br />

in spection to be carried out.<br />

Below there are lists which show examples of such equipment, but<br />

the inspector always has to decide what equipment is necessary in<br />

each speci fic case.<br />

4.1 Inspection Tools<br />

4.1.1 Personal/protective equipment<br />

It is recommended that the inspector is supplied with the fo llowing<br />

personal equipment:<br />

'"<br />

'"<br />

'"<br />

'"<br />

'"<br />

'"<br />

Boi ler suit<br />

Insulal'ion sui t<br />

Rain suit<br />

Working gloves<br />

Rubber boots/waders<br />

Li fe-jacket<br />

Figure 4. / - / Personal Equipmenl<br />

In addition the inspector needs to be supplied with the following<br />

personal protecti ve equipment:<br />

Personal Safety Equipment<br />

'" Helmet<br />

'" Luminolls wai stcoat<br />

'" Protective shoes<br />

'" Goggles<br />

'" Ear protection<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 25


When there is danger of fa lling from he ights, the inspector<br />

ha s to use equipment to prevent th is. Figure 4.1 -2 shows an example<br />

of such equipment that can be led past a pole without being<br />

detached.<br />

Figure 4.1-2 Equipmel1l to prevent/all<br />

When a number of bridges are to be inspected, the inspector must<br />

always be supp lied wit h all the listed personal and protective<br />

eq uipment.<br />

In other cases the type of equipment must be adjusted to the actual<br />

bridge and the aim o f the inspection.<br />

Ordinary Tools<br />

4.1.2 Ordinary Inspection Tools<br />

The ordinary inspection lools are listed below:<br />

* inspection <strong>for</strong>m, included results of the previous inspection<br />

* As built drawing<br />

* Other relevant drawi!<br />

* Maps, road numbers<br />

* Weather resistant per<br />

and pencils<br />

* Clipboard<br />

* <strong>Handbook</strong> <strong>for</strong> bridge<br />

inspection<br />

* Mobi le te lephone.<br />

Figure 4.1-3 OrdillUlY Inspectioll Tools recommended/or Gei/era/illspection<br />

26<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


4.1.3 Inspection Tools <strong>for</strong> General Inspection<br />

The ordinary inspection equipment is listed below:<br />

Equipment Genera l<br />

Inspection<br />

Inspection fo rm, included resu lts of the previous in speetion<br />

As built drawing<br />

Other relevant drawings<br />

Maps, road numbers<br />

Weather resistant pens and penc il s<br />

Clipboard<br />

<strong>Handbook</strong> <strong>for</strong> bridge inspection<br />

M obi le telephone.<br />

Figure 4.1-4 DIY/iI/my inspection Tools<br />

4.1.4 Inspection Tools <strong>for</strong> Major InspeI< Traffic warning signs<br />

• Dictaphone<br />

'" Video recorder<br />

'" Plumbli nc<br />

• Thennometer<br />

'" Magnifying glass<br />

... Gauge <strong>for</strong> measuring crack widths<br />

'" Sliding calliper.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 27


Fil,,'1lre 4.1-5 £qllipmelll Major Inspec/ion<br />

When carrying olltmajor inspection it is also normal to carry out<br />

different measurements and in vest igations of materials.<br />

In vestigations of concrete are most common.<br />

Measureme nts<br />

Investigation of Concrete<br />

Equipment and tools needed <strong>for</strong> these measurements and investigations<br />

of concrete are:<br />

• Small level<br />

• Levell ing equipmen t<br />

• Straight edge<br />

• Measuring device<br />

• Rebound hammer<br />

• Covermcter<br />

• Phenolphthalein fluid<br />

• Wire brush<br />

• Electric chisel<br />

• Hammer drill, AC- or battery<br />

• Small plastic bags <strong>for</strong> concrete dust<br />

• Water proof markers<br />

• Aggregate <strong>for</strong> AC current<br />

• Dry cement mortar and/or joint seal<br />

• Tools <strong>for</strong> mixing ofmortar<br />

Water.<br />

28<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


4.1 .5 Inspection Tools <strong>for</strong> Special Inspection<br />

In addition to the equipment described <strong>for</strong> major inspection, the<br />

special inspection may require eq uipment to carry out material<br />

examinations to veri fy cause and degree of damage. Tllis equipment<br />

is:<br />

Equipment - Special<br />

Inspectio n<br />

• Un iversal instrument fo r electrochemical potential and resistan<br />

ce mappmg<br />

• Device <strong>for</strong> con tro l of surface treatment (Measuring thickness,<br />

bond, etc.)<br />

• Concrete core drill<br />

• Magnetic powder eq uipment<br />

• Ultrasonic equipment<br />

• X- ray equipment.<br />

The use of special inspection equipment often requires<br />

special skil ls or certifica tes, thus qualified inspectors must be hired<br />

from specialist or certifying agencies. Ref. also chapter 7 -<br />

"Surveys, Materials Tests and Instrumentation".<br />

4.1.6 Inspection Too ls <strong>for</strong> Major Underwater­<br />

Inspection<br />

The diver has to use diving equipment in accordance with national<br />

regulations.<br />

To carry out the major inspection<br />

under water may require:<br />

Equipment - Unde rwat er<br />

Inspectio n<br />

• Camera <strong>for</strong> under water use<br />

• Video recorder <strong>for</strong><br />

under water<br />

use<br />

• Ranging rods<br />

• 50111 tape<br />

measure, nylon<br />

• Folding ruler<br />

• Levell ing<br />

equipment<br />

Figure 4. 1-6 Eqllipmelll<strong>for</strong> Major Illspectioll Vllder IfI(lter<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 29


In some cases there can be obslacles that prevent inspection of<br />

foundations under water such as fo rmwork, the foundation being<br />

overgrown, etc. In these cases it can be necessary to use heavy<br />

equipment/tools such as:<br />

Equipment <strong>for</strong> removal<br />

of Formwork<br />

• Lorry equipped with a crane or winch<br />

• Hydraulic tools<br />

• Hydraulic aggregate<br />

• Water jetting equipment<br />

• Barking spade<br />

• Iron bar<br />

• Crow bar<br />

• Axe.<br />

4.1.7 Inspection Tools <strong>for</strong> Major Cable·<br />

Inspection<br />

When carrying out a major inspection of cables it wi ll in most<br />

cases be sufficient to use the same eq uipmen t as fo r major inspection.<br />

4.2 Access Eq u ip m ent<br />

The choice of access equipment when carrying out a bridge<br />

inspection will depend upon the type of inspection and bridge, the<br />

pattern and density of traffic and the total economy of the inspection.<br />

Access Equipment -<br />

General Inspection<br />

4.2.1 Generallnspection<br />

When carrying out general inspection it is not necessary to use<br />

hcavy access equipment like bridge li fts etc, but it may sti ll be<br />

necessary to use light equipment listed below in order to perfonn a<br />

visual check of important construction elements.<br />

• Keys to doors and gatcs<br />

• Under water viewer<br />

• Necessary access equipment to reach specified bridge elements<br />

or parts of elements.<br />

Accesss Equipment­<br />

Other <strong>Inspections</strong><br />

4.2.2 Other <strong>Inspections</strong><br />

For all other types of bridge inspection it is required that the<br />

inspector is within reach of tile structure. In many cases it will be<br />

necessary to use access equipment such as:<br />

• Ladders<br />

• Ordinary lifts<br />

• <strong>Bridge</strong> lifts<br />

• Boats/pontoons/rafts<br />

• Suspended worki ng plat<strong>for</strong>m s<br />

• Professional mountaineering equipment<br />

30<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


The site conditions may decide which access equipment to be<br />

used. In most cases the best choice wi ll be a bridge lift. When in<br />

use on narrow bridges or during dense traffic, bridge lifts may<br />

restrict the traffic flow. In such cases the inspection shou ld, ifpossib<br />

le, be carried out from a boat, pontoon, raft or an ordinary lift<br />

from underneath the bridge. Suspended working plat<strong>for</strong>ms may in<br />

certain cases be a choice.<br />

It is possible 10 combine different types of access equipment. An<br />

ordinary lift can <strong>for</strong> example be used from a pontoon.<br />

Power lines close to the bridge or the existence of a railroad under<br />

the bridge will often influence upon the choice of access equipment.<br />

During the win ter the inspection can, in some parts of the country,<br />

be carried out from the ice. It is important to first control that the<br />

ice is safe.<br />

In the following chapters different types of access eq uipment are<br />

described.<br />

Ladder<br />

fllSpectiolljrOIll (l<br />

4.2.3 Ladder<br />

For minor bridges or bridges with restricted height, the use of a<br />

ladder may be sufficient to get access. Ladders longer than 4 m<br />

must be secured by appropriate means. Inspectors working alone<br />

are not allowed to work from a ladder.<br />

lifts<br />

4.2.4 Ordinary type of Lifts<br />

Ordinary lifts that operate from ground level with the platfonn<br />

moving upwards may be used <strong>for</strong> inspection of overhead trusses<br />

and overhead crossing bridges. Ordinary li fts may also be useful<br />

<strong>for</strong> inspection of bridges with access fo r the equipment from roads<br />

or other hard surfaces under the bridge. The different types are:<br />

* Telescopic lift with scissors action<br />

* A hydrau lic arm with a basket mounted on trailer to be pulled by<br />

car<br />

* A hydraulic ann with a basket mounted on lorry<br />

Scissor lifts<br />

Bascet lifts<br />

Telescopic lifts with sc issors action have rather large work plat<strong>for</strong>ms<br />

that move vert ically. The vertical reach is limited to between<br />

5 and 10 metres.<br />

A hydraulic arm with a basket mounted on trai ler to be pul led by<br />

car has a vertical reach from 10 to 20 m and a horizontal reac h<br />

from 5 to 10m depending on the size and make. They are more fl e­<br />

xible in use than te lescopic lifts and have a lifting capacity <strong>for</strong> two<br />

persons or one person with some equipment.<br />

<strong>Handbook</strong> <strong>for</strong> Bri dge <strong>Inspections</strong> 31


Figure 4.2-1 Ordillwy Baskel Lift all pOIltOOI1S<br />

A hydrau lic arm with a Basket mounted on a lorry has a vertical<br />

reach from 10 to 45 m and a horizontal reach from 5 to 20 m.<br />

Figure 4.1-3. Smo'f{ Basket<br />

Lift 1I101lllted 011 (J Lorry<br />

4.2.5 Types of <strong>Bridge</strong> Lifts<br />

A bridge li ft is a lift specially designed to inspect the lower parts of<br />

a bridge structure from a basket or plat<strong>for</strong>m lowered down underneath<br />

the bridge deck whi le the operating vehicle still is travell ing<br />

on the roadway. In addition supplementary working envi ronment<br />

and safety requirements may appl y.<br />

Minimum Technical<br />

Requirements of a Bascet<br />

Lift<br />

1) The downward reach should exceed 6 m and the ho riz~nta l<br />

reach underneath the bridge deck should be at least 6- 7 m.<br />

2) The device shou ld be equipped with one basket with a safe wor<br />

32<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong>


king load capacity of at least 300 kg at maximum reach. This<br />

will accommodate 2 persons and sufficient equipment. The bas<br />

ket has to be fitted with automatically vertical adj ustment.<br />

3) Manoeuvring must be possible both from the basket and the dri<br />

vers seat in the vehicle. The basket must be fitted with an emer<br />

gency stop device to freeze any movement immed iately.<br />

4) There must be a fixed means of communication between the<br />

basket and the driver's seat.<br />

5) The vehiele should be able to move during the inspection.<br />

6) The maximum allowable pressure from wheels and support legs<br />

is 0.4 N/mm2. Maximum axle load of8 tons.<br />

7) The bridge lift must be able to work from bridges with up to<br />

10 % longitudinal slope<br />

8) The basket must be fitted with electrical power connection and<br />

li ght.<br />

There are two types of bridge lifts available Ihal fulfillhese<br />

requirements:<br />

* <strong>Bridge</strong> lift with basket<br />

* <strong>Bridge</strong> lift with work platfo rm.<br />

<strong>Bridge</strong> Bascet lift<br />

<strong>Bridge</strong> lift with ba sket is the most common type, see Figure 4.2-4<br />

to 3.2.6. The hori zontall y distance is normally 8-1 0 m, but is<br />

depending of how far down the basket can go and how far from the<br />

edge of the bridge the lorry has to drive.<br />

The largest lifts of this type has a downwards range of up to 20-25<br />

m. NormaJl y the reach is 10 m. Most of this type of bridge li fts<br />

may reach upwards as well, see Figure 4.2-7. A typical work diagram<br />

<strong>for</strong> a bridge lift is shown in Figure 4.2-8<br />

Figure 4.2-4 Small <strong>Bridge</strong> Lift with a Basket<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong><br />

33


Example of <strong>Bridge</strong> Lifts<br />

Figure 4.1-5 MediuIII size <strong>Bridge</strong> Lifill'ilh a Baskel (BI'OIl IO sky/iji)<br />

(Mllllllle/a bridge Lifi)<br />

Figure 4.2-6 Large <strong>Bridge</strong> Lifill'ilh a Baskel<br />

Figure 4.1-7 Large <strong>Bridge</strong> Lifiusedfrom<br />

Ground<br />

34<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> In spections


Work Diagram <strong>for</strong> <strong>Bridge</strong><br />

Lift<br />

,....<br />

' ..<br />


limitations to <strong>Bridge</strong> lifts<br />

It is important to be aware of what limitations there are on the operation<br />

of a certain bridge lift in order to make the proper choice.<br />

The limitations are mainly related to the following conditions:<br />

* <strong>Bridge</strong> type<br />

* Width of the roadway<br />

* Railings and light posts<br />

* TaU piers<br />

* Load carrying capacity ( of different parts of the bridge)<br />

Inspecting different<br />

<strong>Bridge</strong> Types<br />

The largest cantilevered box-girder bridges may have a construction<br />

height of up to 15 m at the piers. In order to inspect the lower<br />

flange of the box-girder in this area a bridge lift with sufficient<br />

reach is required. See figure 4.2-10.<br />

The same requirements as above are va lid <strong>for</strong> the inspection of<br />

arch bridges. See figure 4.2-11 .<br />

Figure 4.2-10 Illspeclioll of call1ilevered Box-Girder <strong>Bridge</strong> (K-lijt<br />

r<br />

Figl/l"c 4. 2-11 hrspeclioll of a COllcrele Arclr <strong>Bridge</strong> (Bl"OlIlo sJ.)'lijtJ<br />

36<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


When inspecting suspension bridges, trusses and arch bridges the<br />

manoeuvrabili ty of the bridge lift is of outmost importance. The<br />

basket must be able to move easily in and out between the vertical<br />

and diagonal elements. See figure 4.2- 12. When inspecting minor<br />

through truss bridges the bracing of the top boom may restrict the<br />

movement of the bridge li ft considerably.<br />

<strong>Bridge</strong> Width<br />

Railings/Light Posts<br />

Figure 4.1-11 Illspeclioll of a Tmss <strong>Bridge</strong> (K-lifi)<br />

The space needed <strong>for</strong> the different types of bridge lifts when the<br />

supporting legs are in place varies and has to be considered, especially<br />

on narrow bridges, in order to cause as few problems <strong>for</strong> the<br />

traffic flow as possible.<br />

When footwalks are separated from the roadway by rai ling, this<br />

may influence the required range oflhe bridge li ft in ease it has to<br />

be used from the roadway only. Moving past light posts may hamper<br />

the speed of the in spection considerably. There are bridge lifts<br />

in the marked suitable <strong>for</strong> pass ing light posts and other obstructions<br />

without delay, see Figure 4.2-13.<br />

Figure 4.1-13 Passing a Flagpole (Nummela Brulifi)<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 37


Passing Tall Piers<br />

The access to tall piers may in some cases present a challenge<br />

because reach of the largest lifts is limited. A few of the bridge lifts<br />

may be fitted with a light suspended working plat<strong>for</strong>m, or similar<br />

device underneath the main working plat<strong>for</strong>n1 or basket. See figure<br />

4.2-14.<br />

Figure 4.2-14 Inspection o/Tall Piers<br />

load Carrying Capacity<br />

Pa int Wagon<br />

The load canying capacity of the bridge may in certain cases prohib<br />

it or restrict the use of bridge lifts. It should be noted that that<br />

the pavement may not allow the same loads as the rest of bridge.<br />

<strong>Bridge</strong> lifts or their supporting legs should not be placed on pavements<br />

unless it has been checked thai the pavement is able to cany<br />

the loads in question.<br />

4.2.6 Other types of Access Equipment<br />

Some bridges are fitted with integrated access and maintenance<br />

carriages that can travel underneath the bridge. See figu re 4.2- 15.<br />

Figure 4.2-15: Inspectioll/rom Maintenance Carriage<br />

38<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


Suspended Working<br />

Plat<strong>for</strong>m<br />

Also suspended working plat<strong>for</strong>ms can be used <strong>for</strong> inspection, see<br />

fi gure 4.2- 16. In spection from thi s kind of more stationary equipment<br />

may be an alternative in cases when disturbances to the traffi<br />

c must be avoided. The inspection can not be per<strong>for</strong>med as fast as<br />

with a proper bridge lift, especially if a number of verti cal members<br />

or light posts influence shifting of the equipment.<br />

Figure 4.2-/6: Inspec/ion from a Sllspende(/ Working Plat<strong>for</strong>m<br />

Mountaineering Equipment<br />

Inspection using professional mountaineering equipment may in<br />

some cases represent the only economic alternative to get close<br />

enough to the bridge elements. This alterna tive is not recommended<br />

<strong>for</strong> normal inspection tasks. Such mountaineering equipment<br />

is considered as personal safety equipment and the use and maintenance<br />

is the responsibility of the person to whom it has been issued.<br />

Figure 4.2-17: Inspectioll<br />

/Ising Professio!!al<br />

Moul/tail/eering £qllipll1elll<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong><br />

39


40 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


5 Damage<br />

Evaluation<br />

Fundamentals<br />

5.1 General<br />

When evaluating a damage on a bridge the fo ll owing must be decided:<br />

Basis <strong>for</strong> Evaluation<br />

of Damage<br />

Types of Oa mage<br />

• Dclcnninc the Type of Damage<br />

• Detennine the Consequence of Damage to the bridge<br />

• Dctcnnine the Cause of Damage<br />

In most cases the evaluation ofa damage consists of a visual<br />

check, sometimes followed by measurements and ma.terial investigations.<br />

However, in some special cases, it may be necessary to<br />

carry out calculations of structural capacity, economical considerations<br />

and/or in vestigation by implementing long lenn instrumentati<br />

on survey on the bridge in order to establish rel iab Ie in<strong>for</strong>mation<br />

to evaluate the damage correct.<br />

Deg reel Consequence<br />

of Damage<br />

Cause of Damage<br />

In order to established a unified description of damag e, the listed<br />

types of damage in chapter 5.2 have to be used.<br />

Any damage to be recorded shall be assessed by consjdering the<br />

degree of damage and the consequence of damage.<br />

As part of a complete damage evaluation, al so the cause to the<br />

damage has to be determined. The most common causes of damage<br />

are li sted in chapter 5.6.<br />

5.2 Types of Damage<br />

The most common "Types of Damage" are listed below with a<br />

brief explanatory text connected to each of them. A more extensive<br />

and detailed description of each type of damage inelu sive examples<br />

are given in chapter 9 The Damage Evaluation Catalogue.<br />

Each type of damage is given a three-digit code where the first<br />

digit indicates the material or element the damage referred to, and<br />

the second and third indicate the type of damage. This in order to<br />

ease the registration of damage in the data base, and make it possible<br />

to scan the data/and make statistics. It should be noticed that<br />

one defect may consists of several Types o f Damage.


Da mage typical to Ground<br />

Damage to Ril.'er COllrse<br />

101 Subsidence of • Vertical movement of the ground or<br />

ground/embankment<br />

embankment<br />

102 Obstruction of waterway • When the waterway is partially or totally<br />

blocked<br />

103 Scouring/erosion of river • Removal of soil in river bed area caused by<br />

course<br />

the stream flow<br />

104 Inadequate clearing • All kinds of unwanted vegetation, stones,<br />

up/removal<br />

sand etc. in the river course or items stored<br />

under the bridge<br />

Depositing of mud Is and in river bed<br />

105 Silting up •<br />

106 Insufficient discharge capacity • When the volume of water per unit oftime<br />

flowing under lhe bridge is less than<br />

necessary<br />

107 Change of ri vcr course • When the river flows outside its natural<br />

course<br />

109 Other type of damage to river<br />

course<br />

• Any other damage not li sted here<br />

Damage to protection<br />

facilities:<br />

III Wash out of protection facil ity<br />

• When the stones <strong>for</strong> the rip rap are washed<br />

away<br />

11 2 Scouring of protection • Removal of soil under protection facility<br />

facilities<br />

caused by the water flow<br />

11 3 Movement of protection • The protection facility has moved<br />

facility<br />

horizontally or vertically<br />

114 Defective part of protection • Part of the protection facility is not working<br />

facility<br />

in accordance with expectations<br />

119 Other damage to protection • Any other damage not listed here<br />

facility<br />

2 Damage to Concrete<br />

Elements<br />

20 1 Settlemcnt o f concrete element • Vertical movement of element<br />

202 Movement of concrete • Rotation/dislocation of element(s) from its<br />

element<br />

original position<br />

203 Defonnation of concrete • Loss of original shape or geometry. Includes<br />

element<br />

buckling, bending etc.<br />

204 Cracks in concrete element • Includes all types of cracks<br />

205 Rupture of concrete element • Broken concrete element, member or post<br />

etc.<br />

206 Damage to the concrete • Damage to any surface treatment on<br />

surface treatment<br />

concrete


207 Leakage/dampness of concrete<br />

element<br />

• When liquid penetrates through the element<br />

208 Discoloration of concrete<br />

element<br />

• Discoloured surface of a concrete element<br />

209 Insufficient/damaged cover of<br />

concrete element<br />

• Less cover than designed <strong>for</strong><br />

210 Weathering of concrete elem. • Normal wear and tear<br />

211 Honeycombing of concrete • Caused by <strong>for</strong> example, insufficient<br />

element<br />

vibration of concrete<br />

212 Delamination of concrete • Separation into concrete layers<br />

element<br />

213 Spalling of concrete clement • Bits of the surface concrete falling down<br />

214 Corrosion of rein<strong>for</strong>cement • Rein<strong>for</strong>cement damaged by corrosion<br />

215 Wash out of concrete element • Removal of particles from the concrete hy<br />

water<br />

216 Inadequate cleaning of • Debris, dirt, vegetation etc. not removed<br />

concrete element<br />

from the element<br />

217 Inadequate clearing<br />

up/removal<br />

• Formwork. bars, strip steel etc. not removed<br />

218 Poor concrete quality<br />

• Quality of concrete lower than can be<br />

accepted<br />

219 Scoring/undermining of • Holes in the ri ver bed or bank under<br />

concrete clement<br />

concrete element caused by the flow of river<br />

220 Missing part(s) of concrete • Originally designed part of an element is<br />

element<br />

mlssmg<br />

290 Other damage to concrete • Any other damage not listed above<br />

element<br />

3 Damage ty pical to<br />

SteellAluminium and Iron<br />

Elements<br />

301 Settlement of steellalum.liron • Vertical movement of the element<br />

element<br />

302 Movement of steellalum.liron • Rotation/dislocation of element(s) from its<br />

element<br />

original position<br />

303 Defommtion of • Loss of originally shape or geometry, i.e.<br />

steel/alum.liron element<br />

buckling, bending, kinks etc.<br />

304 Cracks in steeJlalum.liron<br />

clement<br />

• Includes all types of cracks<br />

305 Fracture of steellalum.liron<br />

element<br />

• When a part ofthe steel element is broken<br />

306 Damage to steel surface<br />

treatment<br />

• Damage to coatings. galvanizing etc.<br />

307 Leaks/dampness impact of • When a steel element is leaking


steellalum .liron clement<br />

308 Discolouration of • Discoloured surface of clement<br />

steeValum.liron clement<br />

309 Loose connections of • Looseness of bolts, ri vets or any other part<br />

steel/alum.liron element<br />

of steel element<br />

310 Corrosion of steeUiron<br />

element<br />

• Disintegration of the surface through rust<br />

311 Friction/abrasion of<br />

stcellalum .liron clement<br />

• Abrasion behveen parts caused by friction<br />

312 Broken cable strands • When strands of a cable are broken<br />

313 Inadequate cleaning • All kinds of debris, sand etc. on the element<br />

314 Missing partes) on • Part of ori ginally designed member is<br />

steel/alum .liron clement<br />

missing<br />

315 Inadequate clearing<br />

• Formwork or any other unwanted item on<br />

up/removal<br />

the structure<br />

316 Material fault of steel element • Insuffi cient quality of steel<br />

390 Other damage to steel element • Any other damage not listed above<br />

4 Da mage typica l to<br />

StonelMasonry Elements<br />

401 Settlement of stone/masonry • Vertical movement of the clement<br />

element<br />

402 Movement of stone/masonry • When the element has moved from its<br />

element<br />

original position<br />

403 De<strong>for</strong>mation of stone/masonry • Loss of original shape or geometry, i.e.<br />

element<br />

buckling, bending, etc.<br />

404 Cracks in stone/masonry<br />

element<br />

• Includes aJ l types of cracks<br />

405 Leakage/dampness of<br />

stone/masonry clement<br />

• Leaks through portion of an clement<br />

406 Discoloration of • Discoloured surface of a stonclmasonry<br />

stone/masonry clem.<br />

element<br />

407 Displaced stones in stonework • Slippage of a stona1 portion of the element<br />

408 Collapsed stonework<br />

• When a part of or the entire element has<br />

collapsed<br />

409 Inadequate cleaning of • All kinds of debris, sand etc. on the element<br />

stone/masonry element<br />

410 Inadequate clearing • Fonnwork or any other unwanted item on<br />

up/removal<br />

the structure<br />

411 Wearing of pointing<br />

• Deterioration of mortar in the joints<br />

490 Other damage to • Any other damage not listed above<br />

stone/masonry clem.<br />

5 Damage typical to T imber<br />

Elements


501 Settlement of timber element • Vertical movement of the element<br />

502 Movement of timber clement • When the element has moved from its<br />

original position<br />

503 Defonnation of timber • Loss of original shape or geometry, i.c.<br />

element<br />

buckling, bending, etc.<br />

504 Cracks in timber element • Includes all types of cracks<br />

505 Fracture of timber element<br />

• A broken member of the timber element<br />

506 Damage to timber surface • Damage to painting, impregnation etc<br />

treatment<br />

507 Leakage/dampness of timber • Unwanted leakage through or from an<br />

element<br />

element<br />

508 Discoloration of timber<br />

element<br />

• Discoloured surface of a timber element<br />

509 Chipping & splintering of<br />

timber<br />

• Splintering of timber surface<br />

510 Timber decay • Deterioration of the timber leading to<br />

softness<br />

511 Inadequate cleaning of timber<br />

clement<br />

• All kinds of debris, sand etc. on the element<br />

512 Missing partes) on timber<br />

element<br />

• Lack of any originally designed partes)<br />

513 Loose connections of timber • Looseness of bolts, rivets or any other<br />

element<br />

member<br />

514 Delamination of timber<br />

element<br />

• Separation into layers<br />

590 Other damage to timber<br />

element<br />

• Any other damage not listed above<br />

6 Damage typical to Deck<br />

Pavement<br />

601 Cracks in the surfacing • All types of cracks<br />

602 Leaks through the surfacing • Leaks through portion of the surfacing<br />

603 Ruts in the wearing course • Channelled depressions of the surfacing<br />

following the wheel tracks<br />

604 Unevenness of the surfacing • Corrugation etc. of the wearing course<br />

605 Cracking/potholes of the • Crazing or irregular shaped, disintegrated<br />

surfacing<br />

areas of the surfacing<br />

606 Blistering (toadstools) of the<br />

• Happens nomlally to the watcr proofing<br />

surfacing<br />

layer<br />

607 Flaking of surfacing • Looseness of portiones) of the surfacing<br />

608 Inadequate cleaning of the<br />

• Debris, sand, gravel etc. on the wearing<br />

pavement<br />

course<br />

609 Sweating of the surfacing • When bitumen penetrates to the surface and<br />

make the wearing course slippy<br />

690 Other damage to the surfacing<br />

• Any other damage not li sted above


7 Damage to Bearings/Joints<br />

Damage to Bearings<br />

701 Bearings out o[position • Abnormal position of bearings<br />

702 De<strong>for</strong>mation of bearings • Abnormal de<strong>for</strong>mation of bearings<br />

703 Cracks & Fissures in bearings • Includes all types of cracks<br />

704 Fracture of bearing member • A part of the bearing is broken<br />

705 Damage to surface treatment • Damage to coatings, galvanizing etc.<br />

ofbcarings<br />

706 Corrosion of bearings<br />

• Disintegration of steel surface through rust<br />

707 Inadequate cleaning of • Debri s, sand, gravel etc. on the bearing shelf<br />

bearinglbearing shelf<br />

708 Missing partes) of bearing • Part of original design missing<br />

709 Other damage to beari ngs • Any other damage not listed here<br />

Damage to Joints<br />

711 Abnormal movement of joint • The expansion and contraction behaviour of<br />

the joint is not in accordance with the design<br />

712 Cracks & Fissures in joint • Includes all types of cracks<br />

713 Fracture of joint part • Broken part(s) of the joint<br />

714 Leakage of joint<br />

• The joint is not water tight<br />

715 Corrosion of joint • Disintegration of steel surface through rust<br />

716 Unevenness of joint • Height difference between the joint and the<br />

approaching deck<br />

717 Crackinglholes in joint • Cracking only nonnally appears in asphalt<br />

joints<br />

718 Inadequate cleaning of the • Debris, sand, gravel etc. collected in the<br />

joint<br />

joint<br />

719 Missing part(s) oflhe joint • Part of original design mi ssing<br />

720 Loose part(s) oflhe joint<br />

• Looseness of bo lts, cover plate or any other<br />

part oflhejoint<br />

790 Other damage to the joint • Any other damage not listed here<br />

8 Damage to<br />

Drainage/Approaches and<br />

Accessories<br />

Damage to tile Drain System<br />

801 Defective drain pipes<br />

• Pipes not functioning as planned<br />

802 Leakage o f drain pipes<br />

• Leakage oflhe drain pipe or through the<br />

joint between the pipe and the deck<br />

803 Corrosion of drain pipes<br />

• Disintegration o f pipes through corrosion<br />

804 Inadequate cleaning of the<br />

• Debris, sand, gravel cte. in the drain system,<br />

drain system<br />

but not blocked<br />

805 Blockage of drain system<br />

• Does not allow water to pass<br />

806 Missing part of drain system<br />

• Originally part missing


809 Olher damage to the drain<br />

system<br />

• Any other damage not listed here<br />

Damage to the <strong>Bridge</strong><br />

A pproaches<br />

811 Settlement/subsidence of the<br />

bridge approach<br />

• Depressions in the road surface approaches<br />

812 Potholes in bridge approaches<br />

• Irregular shaped, disintegrated areas orthe<br />

approach road surface<br />

813 Erosion of bridge approaches • Materials removed from the slopes of the<br />

embankment, normally caused by flowing<br />

water<br />

8 14 Extensive vegetation • Vegetation reducing the traffic safety<br />

8 15 Defective drain ditches • Drain ditches arc not functioning as<br />

intended<br />

816 Loss of road camber • Improper cross fa ll of the road surface<br />

819 Other damage to bridge<br />

approaches<br />

• Any other damage not listed here<br />

Damage to Accessories<br />

821 Defective or missing sign(s)<br />

• Sign damaged or mi ss ing<br />

822 Damaged insulation on • Water pipes, electric cables etc.<br />

accessories<br />

829 Other damage to accessories<br />

• Any other damage not listed here<br />

990 Olher da mage to tbe bridge • Any other damage to the structure not listed<br />

in this section


5.3 Degree of Damage<br />

Consequence of<br />

Damage<br />

Degree of Damage<br />

The Degree of Damage is used to indicate the seriousness or severity<br />

of the damage which depends on the development speed and<br />

the rate of severity at the inspection time <strong>for</strong> each indiv idual damage<br />

or group of damage. Four characters indicate di fferent levels of<br />

seriousness of a damage as outlined below:<br />

Degree of Damage ­<br />

Condition<br />

that releases Maintenance<br />

Action<br />

I :<br />

2:<br />

3:<br />

4:<br />

9:<br />

Minor damage or defects that might not require any<br />

remedial action within the next 10 years.<br />

A verage or slight damage or defects that require<br />

remedial action within 4 - 10 years.<br />

Serious damage or defects that requ ire remedial<br />

ac tion within I - 3 years.<br />

Critical damage or defects that require remedial action<br />

within 0 - 1/2 year.<br />

Not inspected<br />

The objective of these characters is to let the inspector indi cate,<br />

the seriousness of the damage observed, based on hi s professional<br />

judgement, and when they have to be repaired.<br />

If the damage may affect the carrying capac ity, thoroughly static<br />

calculations may be necessary in order to determine the severity<br />

be<strong>for</strong>e the degree of damage settles.<br />

When the damage affect the maintenance costs severely, and the<br />

extent is exten sive, a cost benefit analysis should preferably be<br />

carri ed OUI on the bridge be<strong>for</strong>e the degree of damage detennines.<br />

When inspecting a bridge, the inspector has to detennine if the<br />

present condition of the bridge has reached a level where maintenance<br />

action is rel evant or not. The way of doing this <strong>for</strong> the<br />

inspector, is as follows:<br />

Degree of damage 1 is a state of condition which can be accepted<br />

without any recommended action.<br />

Degree of damage 2-4 is a state of condition which demand action.<br />

The inspector has to detennine if degree o f damage 2, 3 or 4<br />

shall be selected, combin ed with recommended year of action to<br />

avoid that the carrying capacity, traffic safety etc. sha ll be affected<br />

seriously.<br />

Conseqence of Damage<br />

The consequences of damage indicate what it will affect if the<br />

damage is not repaired in time. Three effects have been considered<br />

and are abbreviated by letters as fo llows:<br />

C :Damage or defect that affects carrying capacity<br />

T:Damage or defect that affects traffic safety<br />

M: Damage or defect that affects maintenance cost<br />

E: Damage or defect that affects the environment/aesthetics


These effects are presented in order of importance. Damage that<br />

affects carrying capacity, will there<strong>for</strong>e be given higher priority<br />

than that affecti ng environment or maintenance costs.<br />

When relevant, the cost of repairs shall also include traffic costs as<br />

wei l.<br />

One damage may have several consequences.<br />

Assessment of Damage by<br />

Combining Degree and<br />

Consequence of Damage<br />

Damage that affects the<br />

Carrying Capacity<br />

The condition of a bridge element is assessed by cOllS idering the<br />

seriousness and effect of any damage to it. The assessment therefo<br />

re, is a combination of the degree and consequence of the damage.<br />

This combination results in the final assessment ofthc damage as<br />

outlined below:<br />

I C = Minor damage/defect that in the long run may present<br />

danger to the carrying capacity of the structure. The<br />

damage might not require repair within the coming 10<br />

years.<br />

2C = Average damage/defect which can reduce the carrying<br />

capacity of the structure ifno repair is carried out within<br />

the next 3-10 years. The damage must be repaired within<br />

3- 10 years.<br />

3C = Serious damage/defect which can rcduce the carrying<br />

capacity of the structure ifno repair is carried out within<br />

the next 1-3 years. The damage must bc repaired within<br />

\-3 years.<br />

4C = Critical damage which has reduced or is about to reduce<br />

the carrying capacity of the structure. The damage must<br />

be repaired immediately or within half a year if safety<br />

precautions shall be avoided. Report on the findings<br />

shall be submitted to the <strong>Bridge</strong> Engineer immedia<br />

tely.<br />

Damage influencing the<br />

Traffic Safety<br />

Damage inftuencing the<br />

Maintenance Cost<br />

lT ~<br />

2T ~<br />

3T ~<br />

4T ~<br />

lM ~<br />

Minor damage/defect that might in the long run present<br />

danger to the traffic safety. The damage m ight not requi<br />

re to be repaired within the coming 10 years.<br />

Average damage/defect which can reduce the traffic<br />

safety if no repair is carried out within the nex t 3-1 0<br />

years. The damage must be repaired withill 3- 10 years.<br />

Serious damage/defect whi ch can reduce t he traffic safe<br />

ty lfno repair is carried out within the nex t 1-3 years.<br />

The damage must be repai red within 1-3 years.<br />

Critical damage which has reduced or is about to reduce<br />

traffic safety. The damage must be repaired immediately<br />

or wi thin half a year if safety precautions s hall be avo<br />

ided.<br />

Report on the findings shall be submitted to the<br />

<strong>Bridge</strong> Engineer immediately.<br />

Minor damage/defect that in the long run, is considered<br />

to influence the maintenance costs. The damage mi gh t<br />

not require to be repaired with in the coming 10 years.


2M = Average damage/defect that can develop in such a way<br />

that repairs will be more comprehensive, compl icated<br />

and costly ifnothing is done within the next 3- l 0 years.<br />

The da mage must be repaired within 3-10 years.<br />

3M = Serious damage/defect that can develop in SUcJlI a way<br />

that repairs will be more comprehensive, complicated<br />

and costly ifnothing is done within the next 1-3 years.<br />

The damage must be repaired within 1-3 years.<br />

4M = Critical damage that can develop in such a way that<br />

repa irs wil l be more comprehensive, complicated and<br />

costly ifrepair to the damage is not carried out im medi a<br />

tely or within half a year.<br />

Da mage influencing<br />

Environment! Aesthetics<br />

1 E = Minor damage/defect that might in the long rUTh effect the<br />

environment/aesthetics. The damage might not require to<br />

be repaired within the coming 10 years.<br />

2E = Average damage/defect that can develop in such a way<br />

that envi ronment/aesthetics can be effected adversely<br />

within the next 3- 10 years. The damage must be repai red<br />

within 3- 10 years.<br />

3E = Serious damage/defect that can develop in suclll a way<br />

that environment/aesthetics can be effected adverse ly<br />

within the next 1-3 years. The damage must be :repaired<br />

within 1-3 years.<br />

4E = Critical damage that already has nega ti ve impact on<br />

environment/aesthetics or wi ll have withi n 0- 1 (2 year if<br />

the damage is not being repaired immediately or withi n<br />

haifa year.<br />

Examples of damage/defects that affect the Environment/-Aesthetics<br />

can be like noisy joints, painted surfaces with graffiti etc ..<br />

When evaluating a damage determining the consequen ce 10 affect<br />

the Environment/Aesthetics, the Type of Damage is rar ely rated to<br />

be4.<br />

5.4 Damage Evaluation<br />

5.4.1 Primary & Secondary Damage<br />

Sometimes a damage(primary damage) can init iate oth er types of<br />

damage (secondary damage).<br />

Below are listed examples of typical primary damage followed by<br />

some examples of initiated types of secondary damage.<br />

* Settlement of abutment or piers will normal ly lead to de<strong>for</strong>ma<br />

tion of superstructure fo r contin uous bridges.<br />

* C racks in concrete will normally lead to lea kage, stains, disco<br />

loration etc.<br />

Splits in timber may lead to timber decay<br />

* Insufficient covering wi ll normall y lead to corrosion on rein<br />

fo rcemenl or spalling.


The Development o f<br />

Damage<br />

It is important to fully realise the relationship between primary and<br />

secondary damage when both evaluating the damage and decidi ng<br />

the type ofrepair(s).ln most cases primary damage has to be<br />

detennined be<strong>for</strong>e any remedial action can be taken. Repai rs deduced<br />

from secondary damage are rarely successful.<br />

5.4.2 The Extent to which Damage has<br />

Developed<br />

It is usually easy to come to a concl usion about serious damage<br />

which has already reduced carrying capac ity or traffic safety when<br />

remedial measures require to be speedil y set in motion.<br />

Measu rements/Materials<br />

Testing<br />

The Co urse of Development<br />

of Specific Damage<br />

On the other hand it is more difficult to evaluate damage which is<br />

sti ll developing. In such instances it is important to produce a<br />

detailed overview of the following circumstances:<br />

I. How long has it taken <strong>for</strong> the damage noted to develop?<br />

2. How quick is the probability that it will continue developing in<br />

the future?<br />

Observations recorded during previous inspections wi ll be valuable<br />

in connection with assessing how quickly an incidence of<br />

damage has been developing.<br />

In order to assist in assessing the development of damage measurements<br />

and materials testing can additionally undertaken. As an<br />

example, levelling can be employed in recording the development<br />

of settlement, whilst measuring the depth of carbonisation and<br />

chl oride content over a period can be used in evaluating the ri sk of<br />

the re in<strong>for</strong>cement corroding in the fut ure.<br />

In addition to practical experience theoretical models exist <strong>for</strong><br />

assessing the speed at which carbonisation and chlorides are spreading<br />

when it comes to Slating how quick ly specific damage will<br />

continue to develop.<br />

When evaluating the speed of damage destruction one should particu<br />

larly note that different kinds of damage take different courses:<br />

• No development<br />

• Decl ining course of development<br />

• Steady pace of development<br />

• Accelerating pace of development<br />

No Development<br />

Figure 5.4-1 ill ustrates these points. The following sub-secti ons<br />

provide more detailed descriptions of the different courses of<br />

development.<br />

An exampl e could be spalling due to traffic impact. This can arise<br />

quite suddenl y, yet does not develop any further. The damage is<br />

either so immaterial that no action need be taken or so serious that<br />

immediate measures are required. One should, however, real ise<br />

that minor damage to concrete and steel due to traffic impact that<br />

is not repaired in the long run can later lead to secondary damage<br />

such as corrosion.


Declining Course of<br />

Development<br />

Steady Pace of Development<br />

Accelerating Pace of<br />

Development<br />

This can be exempli fied by settlement whi ch usually develops<br />

quickly at the start and then later begins to decline. Nevertheless<br />

one should be aware that settl ement can demonstrate both a steady<br />

and an accelerating course of development.<br />

Rutting can act as an example here. Its development wi ll usuall y<br />

be linear, but an increase in wear and tear must be reckoned with<br />

when the ruts become deeper because traffic impact wi ll be more<br />

concentrated.<br />

Examples of this kind of damage are insufficient surface<br />

cover/damaged cover, secondary damage such as rein<strong>for</strong>cement<br />

corros ion or spal1ing. Since the cover has become carboni sed or<br />

infected with chlorides, the corrosion process wi ll start in the rein<strong>for</strong>cement<br />

clements with least cover with the consequent development<br />

ofspal1ing in the area of these steel elements. As the extent<br />

of the carbon isation or the effects of the chlorides penetrate deeper<br />

into the concrete, so the speed of corrosion development in the<br />

already corroded rein<strong>for</strong>cement elements wi ll increase, and the<br />

corrosion wi ll spread to new rein<strong>for</strong>cement. As a consequence<br />

both corrosion in the rein<strong>for</strong>cement and flak ing will demonstrate<br />

an increasing trend.<br />

Inspection<br />

I<br />

InspeCtion<br />

I<br />

Time I<br />

to Concrete J<br />

== I<br />

I<br />

I<br />

SetUemenl<br />

I<br />

I<br />

o<br />

CotliSion<br />

I<br />

I I J Critical ConOition<br />

----,- --~------<br />

I<br />

I<br />

L -1_ - - - - - - , ____ _<br />

Figure 5.4-1: The Development o/Damage<br />

5.4.3 Compound Damage<br />

Damage to bridges is often composed of severa l types of damage.<br />

Corrosion of rein<strong>for</strong>cement elements often occurs together with<br />

spalling and insufficient/damaged cover.


Whatever types of damage are observed should be used to describe<br />

them, but their assessment shou ld be carried out as a totality. For an<br />

example please refer to Figure 5.4-2.<br />

- -<br />

•<br />

. --.<br />

~-<br />

, ~ - ~<br />

-<br />

\ .<br />

\<br />

•<br />

I "; / /<br />

--'-<br />

Figllre 5.4-2: InsufJiciell//damaged Cover. Corrosion /0 Ille Rein/oreemenl (111(/<br />

Spalling.<br />

The damage illustrated in Figure 5.4-2 consists of insufficient/damaged<br />

cover, corrosion to the rein<strong>for</strong>cement and spalling. Such compound<br />

damage can be assigned different degrees of damage f or carrying capacity,<br />

maintenance costs, the environment and the bridge's overall appearance.<br />

The table be low provides an example of how to describe and<br />

present specific damage.<br />

Evaluation of Compound<br />

Damage<br />

Descri tion of the Dama e C T M E<br />

Insufficient/damaged cover, oorrosion of the rein<strong>for</strong>cement<br />

and spaJlillg on lhe underneath side of the deck. I 2 3<br />

The basis <strong>for</strong> the above damage evaluation is as follows:<br />

The corrosion has occurred in structural rein<strong>for</strong>cemen t but its speed of<br />

development is so low that the carrying capacity wi ll remai n unaffected<br />

<strong>for</strong> the next ten years. A degree of damage of I has been allocated with<br />

respect to cart)'ing capacity (C). The amount of concrete falling off<br />

does not represent any danger to traffic safety (T) since no traffic passes<br />

under the bridge. This column has consequently been left blank.<br />

Even though the speed at which the corrosion is spreading is low, there<br />

exists the probability of the corrosion spreading to several other rein-


fo rcement el ements with a resultant increase in the extent of spa l ~<br />

ling. In tum this will lead to increased repair costs. A d egree of<br />

damage of2 has been given <strong>for</strong> maintenance costs (M).<br />

The bridge is si tuated in an urban environment; consequently s p al~<br />

ling and corroded rein<strong>for</strong>cement present a very unsatisfactory<br />

impression <strong>for</strong> bridge users. A score of 3 has thus beeIll allocated to<br />

environment and overall appearance (E).<br />

5.5 Prioritising<br />

Maintenance<br />

When evaluating damage as already described in Chapters 5.3 and<br />

5.4 it will be possib le in the future to draw up a consciously<br />

thought out prioritisat ion of what damage should be repaired only<br />

once the consequences of possibly de laying maintenance <strong>for</strong> bud~<br />

getary reasons have become known.<br />

However, maintenance should be carried out as and wilen described<br />

in an inspection jfthe damage affects carrying capac ity or traf~<br />

fie safety. Should such maintenance be delayed <strong>for</strong> budgetary<br />

reasons, the consequences may well be a reduction in traffic flow<br />

or the implementation of safety measures.<br />

Additionally when prioritising maintenance one ought to take into<br />

consideration the fact that items of less serious damage can be<br />

delayed if its locat ion allows it to be postponed and easily included<br />

with repairs of serious damage using the same rig or scaffolding.<br />

Table 5.5~ I shows an exampl e of prior it ising and grouping m a int e~<br />

nance tasks as indicated in the previous paragraph.<br />

Priority Element - Damilge Degree of Damage & Time (Of Maintenance<br />

Consequences<br />

I Parapet 4T At unce or within 6 montlt~<br />

- end piece 4T at Lhc:: !~test<br />

Joints<br />

- loose screws<br />

2 Wearing course 3M,2T Ought 10 be carried out<br />

-ru"<br />

within 3 years, hut can be<br />

I OOSIDOnoo a Iitl le<br />

3 ae,~ Ought to be tarried out<br />

- paint damage 2C, 3M within 3 years, but tan be<br />

postponed <strong>for</strong> 4 to 10 years.<br />

Cross girders<br />

All of these elements require<br />

- rdn<strong>for</strong>ccmtnt torrosion maintenaoce simultaneously<br />

2e, 3M as they also need staffolding<br />

Bearings<br />

on the undersid e of the<br />

- cleaning 3M bridge.<br />

- ad iustments 2M<br />

Table 5.5-1: Priori/ising alld GroupingojMaimell(lnce Tasks


5.6 Cause(s) of Damage<br />

The most common causes of damage have been gathered and systematised<br />

using the two digit codes detailed in the foll owing section.<br />

There can be several causes of damage.<br />

Figllre 5.6-1: Hairlinefraell/res &<br />

cmch causetl by Defecl No. 15<br />

Alkalille Reactil'e Materials<br />

Visual checks, suppl emented by measurements and materials testing,<br />

fo rm the basis of determining the cause of damage. However,<br />

a thorough knowledge of tile planning, construction and management<br />

of bridges is also important. The success ofa repair depends<br />

often on correctl y determin ing the primary cause of the damage<br />

when describ ing repairs.<br />

There is no requirement to provide the calise of damage after an<br />

infonnal inspection, but the cause of damage must be given after<br />

all other types of inspection whenever possible.<br />

"-igure 5.6-1: Corroded rein<strong>for</strong>cemenl<br />

due 10 Defect No. 31<br />

Incorrectl), Placetl reillf orcemenl &<br />

No. 34 bwif.jicient Finishing<br />

" ,<br />

Figllre 5.6-3: Hairlille Fractures &<br />

Cm cks dlle to Defect No. 61 Traffic<br />

Loads<br />

Figllre 5.6-4: Gap c(llI.\·el! by traffic<br />

impaci (No. 71)


Cause of Damage<br />

I<br />

Faulty Design<br />

11 lncorrect choice of materials<br />

12 Erroneous calculations<br />

13 Poor design solutions<br />

14 Deviation from standards<br />

15 Inadequate regulations<br />

19 Other fau hy design<br />

2 Material DamagelDefect<br />

21 Poor material composition<br />

22 Inadequate strength<br />

23 Delamination<br />

24 Chloride introduced during mixing<br />

process<br />

25 Alkaline reactive aggregates<br />

29 Other material defects<br />

3 Faulty Construction<br />

31 Settlement of scaffolding<br />

32 Incorrectly placed rein<strong>for</strong>cement<br />

33 Faulty concreting<br />

34 Insufficient finishing<br />

35 Inadequate curing procedures<br />

36 Premature loading<br />

37 Installation fault<br />

39 Other faulty construction<br />

4 Insufficient Maintenance<br />

41 Excessive vegetation<br />

42 Insufficient removal of ice<br />

43 Untimely application of protective<br />

measure<br />

44 Inadequate maintenance<br />

• Wrong materials selected.<br />

• improper or wrong calculations.<br />

• Poor design with regards to maintenance<br />

• i.e. those in <strong>for</strong>ce when the bridge was<br />

constructed.<br />

• e.g. coastal bridges which have been<br />

constructed according to the regulations laid<br />

down <strong>for</strong> inland bridges<br />

• Wrong or improper compositions of materials<br />

or incorrect concrete mix<br />

• Can be like: Poor quality of materials in<br />

taking compression, less tension capacity than<br />

expected, less shear capacity etc ..<br />

• Separation of material into layers.<br />

• Chlorides from aggregates or additives during<br />

the mixing of concrete.<br />

• Aggregate containing alkal ine minerals<br />

• Vertical movement of scaffolding.<br />

• Rein<strong>for</strong>cement not located within the<br />

limitations of tolerance.<br />

• Wrong vibration, to dense rein<strong>for</strong>cement, etc.<br />

• The surface is not in accordance with<br />

requirements.<br />

• Lack of or poor curing lead ing to cracks,<br />

improper quality etc ..<br />

• Loading be<strong>for</strong>e concrete has achieved<br />

required strength.<br />

• Improper installation of a component<br />

• Vegetation growth in river course that can<br />

obstruct the waterway<br />

• Lack of or improper removal of ice<br />

• Incorrcct protection of material<br />

• Maintenance work not carried out in


49 Other insufficient maintenance<br />

5 Environment<br />

51 Chloride loading<br />

52 Sulphate attack<br />

53 Carbonation impact<br />

54<br />

55<br />

56<br />

57<br />

58<br />

59<br />

Leaching<br />

Frost attack<br />

Abrasion<br />

Biological attack<br />

Chemical attack<br />

Other environmental attacks<br />

accordance with regulations/procedures<br />

• From de-icing salt, sea or other salty source.<br />

• Deterioration due to sulfatic acids or materials<br />

• Reaction between the carbon dioxide in the air<br />

and the lime in the building material.<br />

Reduction of the concrete's ability to protect<br />

the rein<strong>for</strong>cement against corrosion.<br />

• When calcium is washed out of the concrete<br />

and deposits as lime on the surface.<br />

• Freeze/thaw cycles that may cause sl'all ing.<br />

Happens normally with porous conc rete.<br />

• Wearing or grinding away of surface material<br />

by water or traffic<br />

• C.g. fungi, maggots<br />

• e.g. acids etc.<br />

6<br />

61<br />

62<br />

63<br />

64<br />

65<br />

66<br />

67<br />

68<br />

69<br />

7<br />

71<br />

72<br />

73<br />

74<br />

75<br />

76<br />

79<br />

Live Loads<br />

Traffic loads<br />

Soil pressure<br />

Impact from currents<br />

Wind impact<br />

Ice impact<br />

Temperature<br />

Shrinkage/Creeping<br />

Impact from overloads on wearing<br />

surface<br />

Other loadings<br />

Accidents<br />

Vehicular impact damage<br />

Impact caused by vessels<br />

Flooding<br />

Landslide! Avalanche/Rockslides<br />

Explosion<br />

Fire attack<br />

Other accidents<br />

• Damage caused by loads from traffic<br />

• Damage caused by soil pressure<br />

• Damage caused by pressure from flowing<br />

water<br />

• Damage caused by wind pressure.<br />

• Damage caused by ice pressure.<br />

• Damage caused by temperature changes<br />

• Time dependent effects which can result in<br />

cracking (shrinkage) and de<strong>for</strong>mation (creep)<br />

• Damage of wearing surface caused by<br />

overloads.<br />

• Damage daused by vehicles.<br />

• Damage caused by vessels when navigable<br />

water under the bridge.<br />

• Damage caused by flood.<br />

• Damage caused by<br />

landslide/avalanche/rockslides<br />

• Damage caused by explosion<br />

• Damage caused by fire.


8<br />

8 1<br />

82<br />

83<br />

84<br />

89<br />

Damage Incurred In Service<br />

Normal wear and tear<br />

Consequential/secondary damage<br />

Impact damage from snow removal<br />

equipment<br />

Vandalism<br />

Other cause to incurred in service<br />

damage<br />

e.g. in the wearing course, surface treatmen t etc.<br />

e.g. de <strong>for</strong>mation of the superstructure due to<br />

settlement, discoloration from leaks and moisture<br />

etc ..<br />

• Damage caused by snow ploughs, graders or<br />

other snow removal tools.<br />

• Damage caused by vandalism<br />

9 Other/U nknown Cause of Damage


6 Carrying out<br />

<strong>Inspections</strong><br />

Ba sis of BRUTUS<br />

Internationa l<br />

Any re levant reports and possibly also drawings should be examined<br />

be<strong>for</strong>e carrying out an inspection with the exception of in <strong>for</strong>mal<br />

inspections.<br />

The access and safety equipment required <strong>for</strong> carrying out a specific<br />

inspection should be detailed in the BMS.<br />

For those bridges recorded in the BMS according 10 given axes<br />

inspection <strong>for</strong>ms should incorporate their elements and the corresponding<br />

axes, -numbers.<br />

The inspection should begin with the lowest axis and progress in<br />

ascending order of axis number. In the absence of classificalion by<br />

axis number in the BMS the inspector should assess whether this<br />

should be introduced.<br />

Systematic Checks<br />

11 is imporlant to inspect bridges in sllch a way that all clemen Is<br />

are checked in a systematic fashion. The following example shows<br />

the possible order in which the elements of a standard, large bridge<br />

could be checked:<br />

I. Ground<br />

2. Substructural elements accessible from land<br />

3. Sub and superstructural elements requiring a bridge lift <strong>for</strong><br />

inspection purposes.<br />

4. Elements belonging to the superstructure which can be in spec<br />

ted from the bridge or the ground<br />

5. Deck, wearing course and accessories<br />

However, the use o f a bridge lift must be assessed in the light of<br />

the above sequence.<br />

Measurementsf M ateria Is<br />

Testing<br />

Pupose of an Inspection<br />

These can be undertaken at the same time as visual checking or be<br />

clearly detailed so that someone else can carry them Ollt. Ifmeasurements<br />

and materials testing have already been planned in advance<br />

of an inspection, these should be specially assessed and adapted<br />

to the findings of the visual check.<br />

The purpose of the different inspections is described in Chapter B<br />

in the "Guidelines fo r the Management of <strong>Bridge</strong>s, whi lst the fo l­<br />

lowing chapters provide a more detailed description of how the<br />

inspections themselves wi ll be carried Ollt.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 59


6.1 Acceptance Inspection<br />

6.1.1 Scope<br />

An Acceptance Inspection incorporates a visual check of the entire<br />

bridge including any underwater foundati ons - please refer to<br />

Chapler 6.6. Cables and their hangers should also be checked <strong>for</strong><br />

suspension and cable-stayed bridges - see Chapter 6.5. Acceptance<br />

<strong>Inspections</strong> should be supplemented by measurements and materials<br />

testing - referto Table 7. 1-\ and Chapters 7.2 - 7.7.<br />

One must be fully aware of the: "Should the owner not advise any<br />

faults di scovered during the <strong>for</strong>ma l acceptance procedures, or<br />

which ought to have been discovered as a result of a customary<br />

careful inspection, he cannot then later plead ignorance of them,"<br />

Damage, faults and defects should be recorded along with their<br />

location. Refer to Chapter 7.1 concerning how to draw up the relevant<br />

reports.<br />

6.1 .2 Visual Checking<br />

This should be carried out at close quarters as described i n Chapter<br />

6.4.2 and should incorporate as a minimum the points lis ted below<br />

<strong>for</strong> indi vidual elements. Please refer to Chapter 9 'Detailed Li st of<br />

Categories of Damage' <strong>for</strong> the assessment of damage.<br />

The Ground<br />

Concrete El ements<br />

* Subsidence of embankment close to abutments, piers and<br />

columns<br />

* Erosion of in fill close to abutments or supports caused by rain<br />

water aC l'ion.<br />

* Materials used <strong>for</strong> ballast are of the prescribed type<br />

• The banks and/or the protection facilities against erosi on com<br />

ply with the description<br />

* Green/planted areas are as ori ginally proposed<br />

* Surrounding areas have been returned to their original condition<br />

• Clearing up operations have been carried out satisfactorily<br />

• Settlement of abutments, piers etc.<br />

• De<strong>for</strong>mation - the shape of the element is correct, e.g. straight<br />

ness/evenness, clearance, defl ection etc.<br />

• Unacceptable hair-cracks/cracks<br />

* Satisfactory quality - thickness, binding agents, evenlless, con<br />

struction - as well as the colour of the surface treatment<br />

• Unacceptable discolorati on due to leaks, dampness impact, cal<br />

cium deposits.<br />

• Insufficient/damaged surface treatment<br />

• Honeycombing or delaminati on<br />

• Spalling due to mechanical impact<br />

• Construction of the concrete's surface is as described<br />

• Formwork removed both from above and below water level<br />

• Nail s and fo rm work stays removed<br />

60<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


o<br />

Fig ure 6.1- 1: Honeycombing<br />

* Holes le ft by stays filled in as described<br />

teel Elements<br />

Timber Elements<br />

Wearing Course<br />

* Settlement or movement in, <strong>for</strong> example, the superstructure<br />

* De<strong>for</strong>mation - the shape of the element is correct, c:.g. straight<br />

ness/evenness, clearance, deflection etc .<br />

• Cracks<br />

* Quality and colour orthe surface treatme nt acceptable<br />

* Surface treatment of mounting joints<br />

* Screws and connections correctly installed<br />

* Transition between the concrete and other material s are as pre<br />

scribed<br />

* As fo r steel elements<br />

* Protection of end pieces<br />

* Dampness traps which can lead to rot<br />

* Correctly prepared so that the timber dries Oul after dampness<br />

impact<br />

* Wearing course and, ifnecessary, the membrane are of the pre<br />

sc ribed type<br />

* Correct thickness - assess need <strong>for</strong> taking measurements<br />

* Finishing edges with joints and raised pavements correctly con<br />

structed<br />

* Depressions - assess need to take measurements<br />

* The drop to the drainage pipe/drain<br />

* Has any damage occurred sllch as fractures and cracks<br />

* Fonnwork, concrete leftovers etc removed<br />

* Cast of pillows underneath bearings correctly carried out wit<br />

hout damage<br />

* Bearing properly located, e.g. facing the correct dir..::ction of<br />

movement<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 61


Bearings & Bea ring Shelves<br />

'" Bearing's positionldefonnation correct in relationship to actual<br />

temperature<br />

'" Protective bellows properly installed<br />

'" Surface treatment as prescribed<br />

Figllre 6.1-2: Too {o w Joilll-Sleeper<br />

Joints & Joint Construction<br />

Pa rapets<br />

Drainage System<br />

'" Formwork removed from joint openings<br />

'" Size of joint openi ngs correct in proportion to the prevailing<br />

!temperature<br />

'" Are the prescribed joint constructions watert ight?<br />

'" Joint sleeper of correct qualit ies and heights<br />

'" Verticall y and horizontall y correctl y shaped<br />

'" Methods of attachment in accordance with regulations<br />

'" Colour and smoothness of surface treatment satisfactory<br />

'" Transition to road guard ra ils carried out in accordanc e with<br />

regulations<br />

'" Corrcct level <strong>for</strong> the upper cdge<br />

'" Sealant around drainpipes and drains sati sfactory<br />

'" Pipe extension below the deck sufficient 10 avoid dam pness<br />

impact to elements located underneath<br />

'" Drain outlets/pipes adeq uately attached and joints tightened<br />

'" Heating cables fu nction as prescribed<br />

6.2 Warranty Inspection<br />

6.2.1 Scope<br />

A Warranty Inspection wi ll incorporate a visual check of the whole<br />

bridge structure as fo r an Acceptance Inspection ~ see C:hapter<br />

6.1. 1. Usua ll y only those measurements and materials testing prescribed<br />

<strong>for</strong> an Acceptance Inspection should be carried o ut. If<br />

damage has occurred during the warranty period Ihe scope of any<br />

measurements and materials testing must be re-assessed ~ refer to<br />

Table 7. 1- 1 and Chapters 7.2 ~ 7.7. For maki ng reports r efer to<br />

Chapter 8.1.<br />

62<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


6.2.2 Visual Checking<br />

The visual inspection should be carried out in the same way as <strong>for</strong><br />

a Major Inspection - see Chapter 6.4.2. Any inspecti ons of the<br />

cables or underwater foundations should con<strong>for</strong>m to Chapters<br />

6.5.2 and 6.6.2.<br />

6.3 Generallnspection<br />

6.3.1 Scope<br />

A General <strong>Inspections</strong> encompasses a simple visual check of all<br />

elements above water level. As much of the foundati ons below<br />

water level should be checked as is possible w ithout employing a<br />

diver. In addition, any specia l checks a lready detailed on (he<br />

inspection fonn should be carried out. Generally speaking, measurements<br />

o r materia ls testing are not required <strong>for</strong> General<br />

<strong>Inspections</strong>. However, the presence of serious rutting may render<br />

measurements necessary to check whether there is a risk of the<br />

dampness insulation being per<strong>for</strong>ated.<br />

The least that must be recorded during a General Inspection is<br />

damage req uiring repair be<strong>for</strong>e the next inspection, i.e. in practice<br />

damage assessed w ith Degrees of Damage 3 and 4. Refer to<br />

Chapter 8.2 <strong>for</strong> the submission of reports.<br />

6.3.2 Basic General I nspection<br />

This is a Basic Visual Inspection without the use of access equipment,<br />

i.e. most of the clements of a large bridge w ill have to be<br />

inspected at a distance. Neverthe less, binoculars should be used<br />

should certain details require to be looked at more closely.<br />

Underwater binoculars may be of assistance when inspecting<br />

items below the surface oftne water.<br />

Ground<br />

During a Visual Inspection each element should be checked<br />

<strong>for</strong> the presence of serious damage - refer to the list below. For<br />

damage assessment please see C hapter 9 Damage Evaluation<br />

Catalogue.<br />

* Settlement o f the ground undemeath the carriageway up against<br />

the abutment piers<br />

* Erosion of the embankment around the abutment pi ers due to<br />

surface water<br />

* More serious underwater damage caused by erosion which can<br />

be detected without using a di ver<br />

* Damage to embankment retaining walls<br />

* Unintentional removal or fi lling up ofloose material in the regi<br />

on of the foundations<br />

* Damming up of driftwood whi ch reduces the water flow<br />

* Unwanted vegetation and trees<br />

* Accumulation of combustible material s under the bridge<br />

* Damage to piles above the waterline<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 63


• Damage to permanent pi lewalls above the water level<br />

Figure 6.3-1: AcculI1ulation of<br />

Twigs and piecesofrree<br />

Figure 6.3-2: End Section of<br />

a Cross-Beam showing broken<br />

off concrete<br />

Concrete Elements<br />

Steel Elements<br />

• Serious sett lement, movement and de<strong>for</strong>mation<br />

• Spalli ng, broken off parts or other damage caused by traffic<br />

im pact<br />

• Discoloration of concrete surfaces due to water or graffi ti<br />

• Unwanted vegetation<br />

• Fonnwork or stays which have not been removed<br />

• General cleaning<br />

• Serious sett lement, movement and de<strong>for</strong>mation<br />

• Defonnation, cracks or breaks caused by tra ffic impact<br />

'" Discoloration due to leaks/dampness impact or graffiti<br />

'" General cleaning<br />

D<br />

Figure 6.3-3: Broken Sleel Girder<br />

64<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


Stone Elements<br />

• Serious settlement/movement of the abutment piers or columns<br />

• Defonnation of stone arches etc.<br />

• Stone slip, stones falling out or missing stones<br />

• Cracked stonework<br />

• Discoloration due to leaks/dampness impact or graffiti<br />

• Unwanted vegetation growth on the element<br />

• General cleaning<br />

Figure 6.3-4: Stonesjallen 0111 ojlhe SIOJlework<br />

Timber Elements<br />

• Serious settlement/displacement of timber columns etc.<br />

• Defonnation of timber superstructure<br />

• Missing parts, braces etc.<br />

• Damage caused by rot<br />

• Chipping or broken off pieces due to traffic accidents<br />

• Discoloration caused by leaks/dampness impact, rust or graffi ti<br />

• General cleaning<br />

D<br />

Figure 6.3-5: ROlto limber Kerb<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 65


Wearing Course<br />

• Ruts<br />

• Cracks or fissures especially around joints<br />

• Crazing or holes<br />

• Flaking off thin wearing courses, e.g. epoxy<br />

• Chippi ng and rot damage (on timber decks)<br />

• Protruding plank ends and nails (timber decks)<br />

FiW-lre 6.3-6: Wear callsetf by Rills<br />

Bearing & Bearing Shelves<br />

Joints & Joint Construction<br />

• Cracks or fissures in sections of a bearing<br />

• Cleaning the bearing and its recess<br />

• Joint anchorage points - possible missing parts<br />

• Mechani cal damage, cracks, breaks in the constructioD due to<br />

sn ow~ c\ eari n g equipment or general wear ca used by tr affic<br />

• Condition of the joint edges & their operation; possibly missi ng<br />

edges<br />

• Cleaning of the joint construction and the gap<br />

Fil:,'1/re 6.3-7: Fixing poinls of a Joilll<br />

66<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


Parapets<br />

* De<strong>for</strong>mation due to traffic colli sions<br />

* Cracks or breaks<br />

* Loose or missing screws, bolts and other parts<br />

* Support struts/posts satisfactorily anchored<br />

* End secti ons and transition/connection to guard rai Ds compl y<br />

with regulations<br />

* General cleaning<br />

* Operating satisfactorily<br />

* Pipes and sand traps are free of blockages and cleaned<br />

Water & Dra inage System<br />

Pipes & Ca bles<br />

Other Equipment<br />

* Leaks and moisture impact (water and sewage pipes.)<br />

* A special list will be produced <strong>for</strong> each bridge<br />

6.4 Major Inspection<br />

6.4.1 Scope<br />

The major inspection consists of a visual inspection o:fthe entire<br />

bridge structure above water except <strong>for</strong> major inspection of cables<br />

described in chapler 6.2. Whenever considered necessary measurements<br />

and material investigations should suppl ement the visual<br />

inspection and serve as a basis <strong>for</strong> evaluation of the fu. ture development<br />

of any observed defects. Reference is made I~ Tab le 7.1-1<br />

and Chapter 7.2 - 7.7.<br />

When great need <strong>for</strong> repair is di scovered during the m.ajor inspection<br />

or when the infonnation gathered is insufficient te decide<br />

what type, degree, consequence, extent or cause of daJl1age that<br />

has been observed, a special inspection mllst be triggered.<br />

Reference to chapter 6.7. Also refer to Figure 6.7- 1.<br />

In the report it should be stated what kind and amount of measurements<br />

and material in vestigations that are needed and <strong>for</strong> which<br />

elements they have 10 be perfonned.<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong><br />

67


For reporting refer to chapter 8.2.<br />

6.4.2 Visual Inspection<br />

The Visual Inspection has to be per<strong>for</strong>med as a close visual inspection,<br />

which means that the inspector must be within reach of element<br />

concerned. This requirement can be suspended provided that<br />

a possible defect can be detected with certainty from a longer di s­<br />

tance. This may be the case <strong>for</strong> inspection of larger uni<strong>for</strong>m steel<br />

or concrete areas. In such cases representative areas should be<br />

selected <strong>for</strong> close visual inspection and the remaining areas left <strong>for</strong><br />

observation from a larger di stance. Hi ghly stressed areas such as<br />

bearings and joints should be subjected to close vis ual inspection.<br />

Serious damage and characteristic defects should be illustmtcd by<br />

means of photographs and lor sketches.<br />

It is necessary to use the appropriate means of access to reach within<br />

the speci fi ed distance of inspection. Reference chapter 4.2<br />

"Access Equipment".<br />

When perfonning the visual inspection all elements shall be surveyed<br />

<strong>for</strong> the existence oflhe following ty pes of damage or<br />

defects. Reference chapter 9 "Catalogue <strong>for</strong> Evaluation of<br />

Defects".<br />

The Ground<br />

• Subsidence of the subso il of the roadway close to the abutments<br />

or in the vic inity of the abutments or supports.<br />

• Erosion of infill close to abutments or supports due to ra inwater<br />

action<br />

• Scouring of river bed<br />

Figure 6.4-/ Erosioll oj£mbal1kmelll<br />

68<br />

Hand book <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


• Damage to slope protection<br />

• Damage to piles above water<br />

• Damage to pennanent sheet piling above water<br />

• Un planned removal or deposition offill material in the vicinity<br />

of foundations<br />

• Accumulation of waste etc. restricting the water flow<br />

• Excessive vegetation, trees etc.<br />

• Accumulation of combustible materials underneath bridges.<br />

Concrete Elements<br />

Steel Ele me nts<br />

• Settlement or movement of abutments, supports, superstructures<br />

etc.<br />

• De<strong>for</strong>mation of superstructure or other element due to differenti<br />

al settlement, excessive load or defomlation of scaffolding<br />

during construction.<br />

• Cracks and possible leakage through these. (It should be eonsi<br />

dered to register crack-widths and crack patterns). Special con<br />

sideration should be given to check anchorage zones of prest res<br />

si ng cables <strong>for</strong> cracks.<br />

* Defect to surface treatment<br />

• Discoloration of concrete surfaces due to leakage or graffiti.<br />

• Reduced or damaged concrete cover with possible future corro<br />

sion damage in mind (carbonisation, ch lorides, binding wire,<br />

di stance holders etc.)<br />

• Disintegration due to frost or weathering<br />

• Pouring defects or areas with obviously bad workmanship, areas<br />

with possible penetration of mo isture, pores in the surface etc.<br />

• Lack of adhesion and/or spalling of structural concrete, integral<br />

ly cast concrete, repaired areas, casting joints, prestressing anc<br />

horages, etc.<br />

• Spall ing, failure or other damage due to coll ision<br />

* Visible rein<strong>for</strong>cement bars or spall ing due to corrosion or woo<br />

den pieces cast into the concrete etc.<br />

• Obvious rein<strong>for</strong>cement corrosion or signs of ongoing corrosion<br />

processes shown by cracking along the outermost rein<strong>for</strong>cement<br />

bars or rust staining.<br />

* Satisfactory concreting around prestressing cable anchorages<br />

• Excessive vegetation, trees etc.<br />

• Scaffolding or ties left in place, etc<br />

• The general state of cleaning o f the considered element.<br />

• De<strong>for</strong>mation of superstructure or other elements due to differen<br />

tia l settlement of foundations, excessive load or col lision.<br />

• Relative movements of superstructure or other elements<br />

• Cracks or fa il ure in base material, welds, bolts or rivets<br />

• Defects in corrosion protection system (paint, galvanising, coa<br />

ting) and possible corrosion. The connection area between cone<br />

rete and steel is especially vulnerable. The same appli es to the<br />

upper flanges supporting wooden roadways.<br />

• Discoloration due to leakage or graffiti<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 69


=<br />

Figure 6.4-2 Rein<strong>for</strong>cement<br />

CorrosiOI/ 011(/ Spallil1g<br />

o<br />

Figllre 6.4-3 DeJeels oil/he Coating Sysrem wilh CorrosiOIl<br />

'" Loose bolts or rivets<br />

'" Missing bolts or ri vets<br />

'" Wear and tear between elements due to movements in_ the bridge<br />

'" Detai ls and profiles with accumulation of dirt and mo:isture<br />

'" General cleaning orthe element.<br />

Stone Elements<br />

'" Settl ements or movements of abutments and supports ,<br />

'" Defonnation of stone arches, etc.<br />

• Split masonry stones<br />

'" Leakage and moisture through abutments, arches etc.<br />

• Discoloration due to leakage or graffiti<br />

'" D isplaced masonry stones<br />

'" Lac king masonry stones<br />

'" Scouring or disintegrati on of mortar in joints<br />

'" Excessive vegetation, trees etc.<br />

• General cleaning.<br />

Figure 6.4-4 Cracks ill Stolles<br />

Timber Elements<br />

• Settl ements or movements of wooden supports, etc.<br />

• Defonnation in wooden sllperstmctures, etc.<br />

70<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong>


• Cracks in timber members<br />

• Splintering or fai lure due to collision<br />

• Defects in surface treatment<br />

• Discoloration due to leakage, moisture, corrosion o:r graffi ti<br />

• Timber decay due to rot or insects<br />

• Lacking parts, shoring, etc.<br />

• Defects in corrosion protection system (paint, galvanising, coa<br />

ting) <strong>for</strong> steel bolts and struts, with subsequent corrosion<br />

• General cleaning.<br />

Wearing Course<br />

• Cracking, especially close to expansion joints<br />

• Leakage or moisture caused by insufficient tightness of the wea<br />

ring surface. (This may result in moist areas and li my deposits<br />

underneath the roadway slab).<br />

• Assessment of wear due to studded tyres, etc. Meas urements<br />

shou ld be considered per<strong>for</strong>med<br />

• Unevenness<br />

• Crackled areas, holes, or bl istering.<br />

• Flaking oflhin wearing surfaces<br />

• Lack of adhesion to base course <strong>for</strong> separately cast wearing sur<br />

faces<br />

• Lack of sealing along edge beams and joints<br />

• Lack of slope towards drain pipes and outlets<br />

D<br />

• •<br />

"!'". ,:-<br />

• •<br />

Figure 6.4-5 Wear (fue 10 siudded lyres<br />

, • •<br />

• Correct thickness of wearing course, to be assessed by measure<br />

ments when required<br />

• Splinteri ng or rot damage (For wooden wearing surfaces).<br />

• Protruding na ils and board ends. (For timber weariDg surfaces).<br />

• General cleaning.<br />

Bearings & Bearing Shelves<br />

• The position of the bearing clements with regard to the actual<br />

temperature, to be measured ifnecessary<br />

• De<strong>for</strong>mation damage to elastomeri c bearing pads<br />

• Cracking or fa ilure to any part og the bearing<br />

• Defects in corrosion protection system (paint, galvanisi ng, coa<br />

ling) and possible corrosion of the bearing.<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 71


I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

Lack of contact in any part of the bearing<br />

Damage to protection cover<br />

Damage to anchor bolts.<br />

Defects in grouts, e.g. cracks, spalling etc.<br />

Damage to concrete bearing seats. Vulnerabl e in case of open<br />

joints in connection with use of dc-icing salt.<br />

Clean ing of bearing and bearing shelv<br />

Joints/Joint Construction<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

>I<<br />

Joint opening related to temperature, to be measured if necessary<br />

Mechani cal damage, cracks, or failure caused by traffi c or snow<br />

plough<br />

Unexpected leakage in waterti ght joints<br />

Damaged or lacking joint threshold<br />

Damaged or lacking anchorage of the joint<br />

Lacking parts in the expansion joint<br />

Blows or noise from the expansion joint when vehicles are pas<br />

sing by<br />

Clean ing status of the expansion joint.<br />

D<br />

Pa rapet<br />

>I<<br />

>I<<br />

>I<<br />

Defonnations due to coll ision<br />

Cracks or failure<br />

Defects in corrosion protection system (paint, gal vanis ing, coa<br />

ting) and poss ible corrosion. Posts are vulnerable where cast<br />

into concrete<br />

D<br />

Figure 6.4-6 RIlPllll'e ofS1eering<br />

Pill oflhe Bellring<br />

Figure 6.4- 7 Missillg ParI<br />

D<br />

Fil:,'1/ re 6.4-8 DlIlI!aged Cooling lind Corrosion<br />

72<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong>


• Discoloration<br />

• Loose or lack ing bolts or parts<br />

• Unsati sfactory connection of posts<br />

• Proper repairs or rein<strong>for</strong>cements per<strong>for</strong>med<br />

• Height in accordance with current regulations<br />

• Ends and transitions to road railing in accordance with current<br />

regulations<br />

• General cleaning.<br />

Drain Pipes and Outlets<br />

Pipes and Cables<br />

Other Equipment<br />

• Pipes and sand traps are open<br />

• Top at corrcct level<br />

• Scaling around pipes<br />

• Offspring underneath structures suffi cient to reduce risk of wet<br />

ting elements underneath<br />

• Defects to pipes such as cracks, corrosion, etc.<br />

• Suspension of drain pipes<br />

• Sealing of joints.<br />

• Damage to fittings<br />

• Damage to insulation<br />

• Leakage of water or sewage pipes<br />

• Unused pipes and cables that may be removed.<br />

• Special checklists to be issued <strong>for</strong> a particular bridge.<br />

o<br />

Figul'e 6.4-9 Corrosion of<br />

Draill System<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong><br />

73


6.5 Major Inspection of Cables<br />

6.5.1 Objective and Scope<br />

<strong>Inspections</strong> incorporate a visual inspection of the load-bearing<br />

cables, suspension rods and retaining elements so as to ensure<br />

these are fulfi lli ng their funct ion. Where necessary measurements<br />

and examination of materials should be undertaken to supplement<br />

the visual check and act as a basis <strong>for</strong> evaluating possible fu ture<br />

damage and wear. See Table 7. 1-1 and Chapter 7.2<br />

It is recommended that a special inspection is carried out whenever<br />

the main cable inspection reveals the need <strong>for</strong> repairs or this<br />

latter inspection has not been suffic ien tly thorough in order to<br />

determine the kind of damage, its consequences, extent or cause.<br />

Refer to Chapter 6. 7 ~ Special <strong>Inspections</strong>. It should be stated<br />

which measurements! materials inspections are to be carried out,<br />

their scope and location. See Chapter 8.2 <strong>for</strong> submitting the relevant<br />

reports.<br />

6.5.2 Visual <strong>Inspections</strong><br />

Visual inspections should be of the close type as detailed in<br />

Chapter 6.4.2 <strong>for</strong> main inspections.<br />

This involves carrying out a closc visual inspection of all cables<br />

from anchorage to anchorage and around the entire cross-section,<br />

and of both the upper and lower suspension<br />

rods and the suspension rod clamps. In special circumstances this<br />

special requirement can be departed from if one can with certainty<br />

detect anticipated damage from a longer distance. Thi s can be the<br />

case with clearly visible lengths of cable or suspension rods. In<br />

such cases representative sections should be selected fo r closer<br />

visual inspection whi lst the remaining areas can be inspected from<br />

greater distances. C haracteristical ly serious damage should be ill u­<br />

strated in photographs or sketches.<br />

Access equipment should be used as required so that one can reach<br />

the prescribed measuring distance. Refer to C hapter 4 .2 - Access<br />

Equipment.<br />

A bridge should be inspected in such a way that a ll its elements are<br />

systematically checked. Cables, anchorages, towers and suspension<br />

rods should be marked with a number which con<strong>for</strong>ms with the<br />

system <strong>for</strong> parts location as detai led in Chapter 2.4.3.<br />

Individual elements are to be checked <strong>for</strong> damage, defects and<br />

fau lts during a visual inspection as listed below. Please refer to<br />

Chapter 9 - Damage Evaluation Catalogue<br />

74<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


load Bearing Cables<br />

• Broken strands. A cable is most subject to broken strands around<br />

the clamps, saddles and anchorage caps. Broken strands can be<br />

identified by longitudinal cracks in the painted surface along the<br />

edges of the broken strands. New brea ks should be marked on<br />

the sketch by specifying the cable number and the approximate<br />

distance from the tower, suspension rods or similar parts.<br />

• Corrosion. Cables should be checked fo r external corrosion and<br />

signs of internal corrosion. This is especially the case with<br />

unprotected cabl es. One indication of internal corrosion can be<br />

an increase in cable diameter.<br />

• Wear and tear/chaffing. Cables are often subj ected to wear and<br />

tear or chaffing around the suspension rod clamps if the suspen<br />

sian rods are hanging out of line.<br />

• Check whether any of the spinning material has begun to leak<br />

out of the inner cable.<br />

• The condition of the surface treatment should be evaluated.<br />

• Check whether there has been any slipping between cables and<br />

their saddles.<br />

• Packing around the saddl es. Ensure that the cables are compl e<br />

tely surrounded by packing material if this has been used and<br />

that the fasteners are in good condition. The packing material<br />

should be soft and elastic and bear no signs of cracks or other<br />

damage.<br />

Figllre 6. 5- /: Broken Strands of a Cable<br />

Saddles/ Bearings of<br />

Main Cables<br />

Anchorage Caps<br />

• Loose/missing bolts, nuts or clamp plates<br />

• Movement<br />

• Cracks<br />

• Corrosion damage<br />

• Condit ion of the surface treatment<br />

• Birds' nests or other <strong>for</strong>ms of surface soiling<br />

• Check that the anchorage caps arc correctly seated on their stays<br />

and that the tangents of the cabl es fonn the correct angles.<br />

• Check whether the cement grouting in the joints betwcen cables<br />

and cable heads is still intact. The grouting should be removed<br />

from a couple of the cable heads of each anchorage. If corrosion<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 75


is discovered in the grouting cement then all joints shou ld be<br />

checked. New cement grouting of the same type should be<br />

app lied to the joints once these have been thoroughly cleaned.<br />

• Check <strong>for</strong> sagging in the cast anchorage cones. This can be iden<br />

tified by the presence o f leaked casting material along the cable<br />

at the entrance to the cable head.<br />

Anchorage o f Ca bles<br />

• Some cable anchorages have been constructed in such a way<br />

that the cable head and parts of the cable have been cast in con<br />

crete. This concrete should be removed in order to release the<br />

cable up to the anchor head <strong>for</strong> inspection.<br />

Figure6.5-2: Cable Heads imbedded ill COllcrete<br />

• Cables/stays slink into weak soi l: an assessment should be made<br />

as to whether a partial excavation should be undertaken to deter<br />

mine their condition. However, excavation work must not in any<br />

way weaken the rivet holders <strong>for</strong> the gravitat ional anchorage<br />

points.<br />

Suspension Rod Clamps<br />

• Movement. The suspension rods should be checked <strong>for</strong> out-of-l<br />

line movement; check also whether the suspension rod plates<br />

have moved in such a way that the suspension rods are touching<br />

or rubbing against the cables.<br />

• Movement. Sagging can arise around the cable suspension rods<br />

between the cables and the cable cap. The cast metal can be<br />

extruded as thin flakes in the joint between the cap and the<br />

cable.<br />

• De<strong>for</strong>med bolts, clamps etc.<br />

• Cracked or broken bolts, clamps etc.<br />

76<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


* Damage to the surface treatment<br />

Figure 6.5-3<br />

Wear& Tear<br />


When an underwater main inspection has revealed the need <strong>for</strong><br />

major repairs or has not been adequate enough to ascertain the<br />

nature of any damage, its consequences, scope or cause, then more<br />

comprehensive measurements and materials testing may require to<br />

be carried oul.<br />

The inspection should be undertaken by di vers who must possess<br />

the necessary quali fications and approval in accordance with<br />

public regulations.<br />

Refer to Chapter 8.2 <strong>for</strong> making reports of Underwater Major<br />

<strong>Inspections</strong>.<br />

6.6.2 Visual <strong>Inspections</strong><br />

These should be made at close quarters, i.e. the diver should be<br />

able to touch the different bri dge elements.<br />

Be<strong>for</strong>e a visual inspection can be conducted all fo rm work and<br />

overgrowth remaining should first be removed from a large<br />

enough area so as to provide a sufficien tl y clear overview of the<br />

condition of the fou ndat ions. The anti-rust protection does not<br />

have to be taken away in order to remove absolutely all the <strong>for</strong>mwork.<br />

Ice Sheath ing does not require to be removed either.<br />

Overgrowth can be removed either with a barking spade orland a<br />

high pressure hose.<br />

In accordancc with Chapter 2.1.6 any damage should be recorded<br />

on fold-out drawings of the foundations.<br />

The foundations should be inspected from the riverbed upwards to<br />

the water surface and include tida l areas. Any damage should be<br />

photographed and described accurately.<br />

Each element is to be inspected <strong>for</strong> damage, defects and faults as<br />

detailed below. Refer 10 Chapter 9, Damage Eva luation Catalogue.<br />

Underwater (; round<br />

Concrete Elements<br />

'" Erosion and lor undermining of foundations<br />

'" Damming up caused by loose material, wood, branches whi ch<br />

can reduce the through flow of water.<br />

'" Damage to free-standing piles<br />

'" Damage to protection agai nst erosion<br />

'" Settlement/movement of abutment pi ers, piers etc.<br />

'" Hair cracks and cracks.<br />

'" Rein<strong>for</strong>cement with little or damaged cover.<br />

'" Weathering due, <strong>for</strong> example, to frost, strain caused by weather<br />

cond it ions etc. especially in areas subject to tides.<br />

'" Depressions/holes in castings or badly cast joints.<br />

'" Corrosion of the re in<strong>for</strong>cement or spalling.<br />

'" Areas subject to wash out.<br />

78<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


Stone Elements<br />

Steel Elements<br />

Timber Elements<br />

* Settlement or movement<br />

* Cracks<br />

* Earth slips, landslides or mi ssing stones<br />

* Pointing which has been washed away or has becom e weathe<br />

red.<br />

* Settlement or movement<br />

* Cracks or breaks<br />

* Corrosion<br />

* Missing support braces/parts<br />

* Damage to cathodic protection<br />

* Settlement or movement<br />

* Cracks or breaks<br />

* Damage due to rotting<br />

* Missing pans/supporting sections<br />

* Corrosion of retaining bolts and steel stays<br />

* Worm infestati on<br />

* Scouring or wear and tear due to ice<br />

Figure 6.6-1 Erosion Gild Scouring<br />

Figure 6.6-2 Fa(led Areas<br />

6.7 Special Inspection<br />

When a special inspection has been initiated as a result ofa main<br />

inspection, the course of the inspection work could be as described<br />

below in Figure 6.7-1.<br />

6.7.1 Scope of Inspection<br />

A Special Inspection should be carried out either ofth.e entire bridge<br />

or only of critically exposed or damaged elements. A Special<br />

Inspection will encompass<br />

visual checks and/or surveys/materials testi ng.<br />

The type and scope of surveys and materials testing w ill be that<br />

stated in earl ier<br />

inspections, but should additionally be evaluated by t he Inspector.<br />

If the Special Inspection has not been in itiated by a previous<br />

inspection, the I<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 79


a'or ns ection<br />

Normal lnspecticn &<br />

Maintenan


6.8 Maintenance Measures -<br />

Extent of Damage<br />

The aim of carrying out maintenance to bridges is to ensure that<br />

the same standards and levels of safety are kept during their entire<br />

planned life.<br />

Agreed Time <strong>for</strong><br />

Maintenance<br />

Description of Measures<br />

Alternative Stratigies<br />

Pro cedural Codes<br />

Repairs to Concrete<br />

Maintenance shal l be carried out when the fo llowing three considerations<br />

coincide:<br />

-a) Costs are at thei r lowest point.<br />

-b) The bridge's carry ing capacity ca n be main tained.<br />

-c) Users are af<strong>for</strong>ded adequate safety and access.<br />

Addi tionally, one must ensure that a bridge does not negatively<br />

affect the environment and surroundings in whic h it is situated.<br />

Whenever a Major Inspection uncovers damage which requires<br />

ma intenance (Degree of damage 2), a descript ion of the required<br />

measures and associated cost overview must be drawn up.<br />

Following either a Major or Special Inspection an evaluat ion of the<br />

possible alternative ma intenance strategies can be undertaken in<br />

accordance with the Norwegian Public Roads Administration<br />

<strong>Handbook</strong> No. 147: "The Management, Running & Maintenance<br />

of <strong>Bridge</strong>s".<br />

The description of the measures to be taken should be based on<br />

procedures which comply with the Norwegian Public Roads<br />

Admi ni stra tion <strong>Handbook</strong> No. 026; " Procedural Codes - 2, 1997".<br />

The materi al s quanti ties incl uded under the different procedures<br />

should be decided on as much as possible at the bridge location.<br />

The extent of, fo r example, mechanical repairs to a concrete bridge<br />

are decided most eas il y by selec ti ng one or more smaller but representative<br />

areas or test sections. Here one can recordfevaluate the<br />

extent of the different kinds of damage.<br />

If the decision is taken to employ special repair methods such as<br />

the following:<br />

- Re-a lkalising<br />

- Chloride extraction<br />

- Cathodic protective measures<br />

then a simultaneous inspection should be carried Oul <strong>for</strong> the presence<br />

of surface impuriti es on, <strong>for</strong> exampl e, metal rein <strong>for</strong>cement<br />

spacers, nails and binding wires, al l of which could affect the technical<br />

and financial measures adopted. In addition, surface impurities<br />

can have an effect on the surface treatment of the concrete.<br />

Re pairs t o Steel<br />

As with concrete bridges it can also be of interest to undertake surveys<br />

of smaller representative sections of steel bridges showing<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 81


evidence of deep-seated corrosion. In this way one can determine<br />

the size of the surface area requiring sandblast ing and the application<br />

of new paint surfaces.<br />

Surface Treatment<br />

The most conveni ent way of calculating the area that and treatment,<br />

is from the original drawings. If these do not exist,measurements<br />

must be per<strong>for</strong>med. In some cases there might be a necessity<br />

of taking samples in order to determine the type of coatings. The<br />

selec tion of repainting system is dependent on the existing coating<br />

system. In most cases it is reasonabl e to paint some test-areas<br />

be<strong>for</strong>e th e final painting system is being determined.<br />

Railings and Parapets<br />

Joints<br />

So far as damage to rai lings or parapets is concerned, measurements<br />

should be taken of the total length in meters of those sections<br />

to be repaired and those to be repl aced. The total number of<br />

posts to be rep laced should also be calculated.<br />

If the renewal of joint sections is considered a possibility, the joint<br />

apertures should be measured and th e temperature recorded. It will<br />

also be necessary to clarify whether the apertures are sufficiently<br />

wide or whether they shou ld be widened/narrowed. In add ition the<br />

length of the joint construction should be measured. A check<br />

should al so be carri ed out to determine whether there are ex isti ng<br />

railing posts which could be in the way of new joint constructions.<br />

Consideration should also be given to the need to jack up/adjust<br />

bearings due to differences in their settings.<br />

82<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


7 Surveys, Materials<br />

Tests & Instrumentation<br />

7.1 General<br />

It may be necessary to supplement visual checks by surveys, mat e~<br />

rials testing and instrumentation in order to find a better basis <strong>for</strong><br />

determining the extent orany damage, its cause, degree and consequences<br />

or <strong>for</strong> uncovering hidden damage.<br />

Scope<br />

The scope of these measurements and investigations must be evaluated<br />

in every case and will depend on:<br />

* The type of inspection<br />

• The type ofhridge<br />

• The type o f materials lIsed<br />

• Wear caused by the climate<br />

• Visual observations<br />

In order to carry out such measurements and in vestigations in a<br />

focused manner one should have a clear picture of their need and<br />

uti litarian value. For the sake of appearance, thi s is advisabl e with<br />

regard to the costs and the possib ly destructive measures employed.<br />

An overview of which surveys and material s testing can be undertaken<br />

in connection with the different types of inspections can be<br />

found in Table 7. 1-1. Provided the prescribed measurements and<br />

materials testing have been documented at the building stage,<br />

these do not require to be repeated <strong>for</strong> a completion survey.<br />

Special Routines<br />

Special routines may have been pu t into effect <strong>for</strong> certain bridges<br />

in connection with surveys, materials testing and/or surveillance<br />

by instruments. This will become evident from the inspecti on plan<br />

in BRUTUS International.<br />

Several of the surveys and materials in vestigations require special<br />

routines and additional quality assurance. Often special competence<br />

and equipment are also needed. Such is always the case <strong>for</strong> the<br />

installation of surveillance instruments. Refer also to Chapler 8<br />

- Reporting of Inspection Results.


TYPE OF INS PECTIONS<br />

0<br />

g<br />

Possible Measurements & Materials Investigations 0<br />

0 '5<br />

"5 0 0 ,<br />

0 0<br />

'5 .2 " 0.<br />

0- ~<br />

= .2<br />

~ 0 ti<br />

0<br />

= .2<br />

0 0. ti<br />

- 'u -<br />

" i\. ti<br />

" " "<br />

'"<br />

~ :0 " " 0-<br />

0 0. o.v ~<br />

0 c - =<br />

" • ~ - 0<br />

0<br />

•<br />

U = • 0<br />

15. r! - " -: ~ -<br />

• " 0 •<br />

" " 0<br />

o " ·0<br />

0<br />

I ~<br />

., 0<br />

0<br />

If . .~"<br />

;;:


All the measurements and materials investigations li sted in Table<br />

7. 1·1 are also described in the "Working procedure Code"<br />

(handbook from NPRA)<br />

Supplementary infonnation can also be found in Chapter 7.2 - 7.8<br />

of this manual. Amongst other things the fo ll owing in<strong>for</strong>mation<br />

has been detailed:<br />

Purpose of such measurements/investigations<br />

Advantages and disadvantages of the different methods<br />

Requ ired eq uipment<br />

Reference to other manuals which can provide more deta iled<br />

infonnation<br />

7.2 Measurements<br />

7.2.1 Levelling<br />

Purpose<br />

Procedures<br />

To measure settlement, movement and defannation and follow up<br />

possibl e developments.<br />

The need <strong>for</strong> levelli ng differs fo r new and older bridges, which is<br />

reflected in the need <strong>for</strong> levelli ng during completion surveys and<br />

other types of inspections.<br />

When measurements are taken on a bridge's superstructure, the<br />

effects of the vibration caused by heavy traffic must be taken into<br />

consideration. If serious vibrations are experienced, measurements<br />

should be taken during periods oflow traffic or while the bridge is<br />

closed <strong>for</strong> this purpose.<br />

Scope<br />

Acceptance Inspection<br />

For each bridge, levelling should be conducted on all axes and<br />

centrall y in each section.<br />

Levelling bolts require to be installed on bridges with foundations<br />

in weak ground. Regular measurements need not n0011ally be<br />

taken <strong>for</strong> bridges whose foundations have been sunk into rock;<br />

neither are levell ing bolts requi red.<br />

A decision must be reached as to whether follow·up is to be<br />

undertaken during the operational phase.<br />

Other <strong>Inspections</strong><br />

Any fo llow·up inspection in the operational phase stipulated<br />

during a completion survey must be carried Olii.<br />

Levelling must be undertaken in the event of settlement, move·<br />

menl or defonnation. Levell ing can be carried out direct ly on the<br />

relevant clements. However, if developments are to be fo llowed<br />

up over a period, then levelling bolts should be installed.


Equipment<br />

* Theodolite<br />

* Tripod<br />

* Levell ing pole<br />

* Measuring tape<br />

* Levelling bolts and hammer action drill, if necessary.<br />

Purpose<br />

7.2.2 Horizontal Distances/Displacement<br />

To measure movement, <strong>for</strong> examp le of abutment piers, piers,<br />

superstructure etc.<br />

Procedures<br />

Reference is made to Procedure Movement. Movement can often<br />

be noted in bearings and joint apertures and can be measured w ith<br />

a folding rule or poss ibly by using a sma ll spirit level. Movement<br />

in piers can be measured with a plumb linc. The measurement o f<br />

movement should be taken in connection with recording the temperature.<br />

Ifmovement has to be followed up over a period bolts<br />

should be installed between which the measurements are to be<br />

taken. In order to determine which parts are subject to movement,<br />

a levell ing instrument can be empl oyed .<br />

.. .<br />

• •<br />

Figure 7.2 ~ I MeaSliremelll of Displacemelll<br />

Acceptance Inspection<br />

sco pe<br />

For all bridges with moving bearings an inspection must be made<br />

of the bearing's placement, orientation and any displacement. The<br />

first two points should specifically be checked against the original<br />

drawings. The joint apertures and their associated temperatures<br />

should also be recorded.<br />

Other <strong>Inspections</strong><br />

The need <strong>for</strong> taking measurements should be assessed in connection<br />

with the visual inspec tion.<br />

Equipment<br />

Purpose<br />

* Fol di ng rul e<br />

* Spirit level<br />

* Plumb and line<br />

* Thennomeler<br />

* Levell ing Telescope<br />

7.2.3 Measuring the Thickness of Wearing<br />

Course<br />

To measure the thickness of the asphalt wearing surface on the<br />

bridge deck to check whether it meets requirements or not.


Procedures<br />

Scope<br />

Equipment<br />

The thi ck ness of the wearing surface may vary in a crosswise<br />

direction <strong>for</strong> bridges on a bend.<br />

Acceptance Inspection<br />

A minimum of three sets of measurements must be taken along the<br />

centre line as we ll as along each side of the bridge at 100 metre<br />

gaps. At least four sets of measurements should be carried out per<br />

bridge.<br />

Measuring the thi ckness of concrete wearing surfaces should be<br />

conducted as <strong>for</strong> locating rein<strong>for</strong>cement elements (See Chapter<br />

7.3.1: Locating Rein<strong>for</strong>cement Elements - Measuring Cover).<br />

Other <strong>Inspections</strong><br />

The need fo r taking measurements should be assessed in connection<br />

with the visual inspection. The scope of the measurements<br />

should be the same as <strong>for</strong> a completion survey.<br />

* Fo lding rul e<br />

* Drill<br />

* Ma terial to refi ll holes<br />

Figure 7.2-2: Measurillg Track Wear<br />

Purpose<br />

7.2.4 Measuring of Ruts<br />

To measure the depth of wear in the tracks created by studded<br />

lyres in the wearing surface.<br />

Reference is made to rel evant procedures.<br />

Scope<br />

Acceptance Inspection<br />

The measurement of track wear is not relevant.<br />

Equipment<br />

Other inspections<br />

When track wear indicates a need <strong>for</strong> taking measurements, measurements<br />

should be made in a minimum of two sections of tile<br />

bridge - one wi th minimal, the other with maximum wear - lIsing a<br />

straightedge. For long bridges over 200 metres, measurements are<br />

to be taken in one section <strong>for</strong> every 100 metres. The depth of the<br />

wear should be recorded crosswise every 250 metres.


A special note should be made whenever track wear is so great that<br />

the dampness insulation material or the bridge dec k have become<br />

visibl e.<br />

Equipment<br />

• An aluminium straight edge rul e<br />

• A measuring wedge<br />

Purpose<br />

Procedures<br />

Scope<br />

Equipment<br />

7.2.5 Measuring Evenness of the Deck Surface<br />

To measure the evenness of the wearing surface of new bridges or<br />

whcnever a new wearing surface has been laid on older bridges.<br />

Reference is made to Procedure 87. 1815. Damage No 604 on page 266<br />

Acceptance Inspection<br />

Measurements fo r evenness can be taken using a straightedge or a<br />

measurement vehi cle. The height of the joint construction should<br />

be checked in relationship to the wearing surface and then recorded.<br />

Other <strong>Inspections</strong><br />

Evenness measurements are not nonnally carried out.<br />

• Straight edge, either 1 or 3 metres long with lugs<br />

• Measuring wedge<br />

Purpose<br />

7.2.6 Measuring Sag<br />

To measure the relative sag in suspension bridge cables in order to<br />

check the loads in the suspension rods.<br />

Relative Sag<br />

Plumb line<br />

Hanger


Procedures<br />

Scope<br />

Sag is measured using cord or possibly piano wire as indicated in<br />

Figure 7.2-3. A bob should be hung on the end of the cord; alternati<br />

vely a spring balance may be used. The vertical distance bctween<br />

the central suspension rod and the taut cord (the amount of sag) is<br />

then measured. The procedure is repeated <strong>for</strong> all suspension rods 0<br />

n both sides o f the bridge. The amount of sag is nonnally the same<br />

over the whole bridge, but can vary somewhat near the towers<br />

because ofthe di stance between the fi nal suspension rod and the<br />

tower, and the tension of the braces. It is important that the bridge<br />

is not subject to traffic loads or lift during measuring.<br />

Acceptance Inspection<br />

Sag should normally be measured in conjunction with the bridge's<br />

construction . However, iflhis cannol be shown 10 be documented,<br />

then these measurements should be taken during the Acceptance<br />

Inspection.<br />

Main Cable Inspection - Special Inspection<br />

The need to take these measurements should be evaluated during<br />

the visual inspection.<br />

Equipment<br />

Purpose<br />

Procedures<br />

Scope<br />

• Cord, possibly piano wire<br />

• Plumb line, possibly a spring balance<br />

• Folding rule<br />

7.2.7 Recording <strong>Bridge</strong> Details<br />

To record:<br />

• mi ss ing data co ncerning elements, element types, size etc.<br />

• marking a bridge<br />

• erecting traffic signs<br />

• bridge drawings (completed drawings)<br />

• archi ve/computer system data<br />

Procedures and eq uipment requirements wi ll vary according to the<br />

task in hand.<br />

Acceptance Inspection<br />

Should data <strong>for</strong> new bridges not have been recorded at the building<br />

stage, then this should be done at the latest during the Completion<br />

Survey.<br />

Major Inspection - Special Inspection<br />

The data in BRUTUS should be checked <strong>for</strong> accuracy. Additional<br />

inspections should be carried out after reconstruction or rein<strong>for</strong>cement<br />

works.<br />

Equipment<br />

• Trip counter<br />

• <strong>Bridge</strong> traffic sign and tools <strong>for</strong> erecting it<br />

• Fo ld ing rule<br />

• Measuring tape<br />

• Camera<br />

• Surveying equipment


7.2.8 Measuring of Vertical Clearance<br />

Purpose<br />

Procedures<br />

Scope<br />

To measure the headroom <strong>for</strong> bridges crossing roads and the clearance<br />

<strong>for</strong> sh ips under bridges over the sea or other water.<br />

A headroom check may become necessary after rcasphalting or<br />

ot her changes to the roadway or, <strong>for</strong> example, after a heavy load<br />

has used the road. Depending on the bridge's design and the purpose<br />

of the measurements it may be relevant to take maximum and<br />

minimum headroom measurements.<br />

Acceptance Inspection<br />

Should the headroom of a new bridge not have been carried out at<br />

the building stage, then this should be done al the latest during the<br />

Completion SUlVey.<br />

Major Inspection - Special Inspection<br />

Headroom should be measured after rcasphalting or other works<br />

which can affect a bridge' s headroom.<br />

Equipment<br />

* Measuring tape<br />

* Telescopic measuring rod<br />

* Surveying equipment<br />

7.3 Adequate Materials<br />

Investigation - Concrete<br />

The following sections provide a description of the materials in vestigations<br />

which can be undertaken during the inspection ofbridges<br />

and their concrete elements.<br />

When evaluating the condition of a concrete construction it is<br />

important 10 remember that the different materials investigations<br />

should be viewed in relationship to one another.<br />

The local ising of materials investigations fo r coastal bridges is<br />

specificall y dealt with in Chapler 7.3.9.<br />

Refilling Test Holes..cuts<br />

Several of the materials investigations carried out on concrete<br />

require the drilling of holes or chiselling out cuts in the concrete.<br />

Procedural Code - 2 lays down a requirement in sllch instances<br />

that the holes/cllts be refilled. However, no guidelines have been<br />

given as to how th is should be completed. The foll owing procedures<br />

have there<strong>for</strong>e been recommended:<br />

Holes of a Diameter < 25 mm<br />

The hol es should be fi ll ed with grey paintable single-component<br />

polyurethane grouting or equivalent cement mortar,<br />

The holes should be completely fi lled using a tube connected to a


grouting gun pushed all the way to the bottom of the hol e. As the<br />

hol e fill s up the tube is gradually removed.<br />

Holes resulting from Core Drilling or larger Chiselled Cuts<br />

Dust and loose particles should be cleaned out with water after<br />

which any water remaining should be dried up . The mortar to be<br />

used <strong>for</strong> the repair(s) should be mixed to the required consistency<br />

and put in the ho le(s) to 2·3cm below the surface level. Once the<br />

mortar has set the remainder of the hole should be fill ed with mar·<br />

tar flush with the surface. Immediately thereafter a layer of thick<br />

elastic cement-based coating should be applied to the surface.<br />

Mortar used to repair holes resulting from core dri ll ing or larger<br />

chiselled cuts should satisfy the same requirements <strong>for</strong> mortar<br />

used during mechanical repairs.<br />

Purpose<br />

Procedures<br />

7.3. 1 Locating the Rein<strong>for</strong>cement - Measuring<br />

its Cover<br />

To locate the rein<strong>for</strong>cement and measure its cover.<br />

Reference is made to the Nonvegian Public Roads Administrati on<br />

<strong>Handbook</strong> No. 015: "Tests carried out in the Field", Method<br />

No. 15.542.<br />

The description given in the procedural code of how cover is measured<br />

should be used to obtain accurate measurements. However,<br />

these can be simpl ified as follows if the measurements are more in<br />

the nature of a spot test:<br />

In the area where the cover is to be measured locate the load bearing<br />

rein<strong>for</strong>cement and the direction in which it is lyi ng. If possible<br />

the nearest mounting rod should also be located<br />

The cover is to be measured <strong>for</strong> a minimum of three rods in the<br />

outennost layer of the load bearing rein<strong>for</strong>cement.<br />

Measurements are to be taken at a point halfway between intersecting<br />

rods (see Figure 7.3- 1).<br />

x<br />

®<br />

x<br />

x<br />

o x<br />

,<br />

Me8wrernent poinllOl I~d l;JeR ri~ reinloroem ent<br />

Outermost layer<br />

of load bearing<br />

rein<strong>for</strong>(lement<br />

>,·-1 . Intersecting Rods: ,....,. ,<br />

• I<br />

Itw! nf!'xt outermo!ll<br />

layer of load bc.aIing ~.<br />

Mounting fl od<br />

,<br />

..,<br />

. . .<br />

" . ,~~ .<br />

, '<br />

,... ......<br />

......<br />

.,<br />

' ~,'\ ~ ....... ,<br />

. ,<br />

. . ,<br />

" •• II' .\, •<br />

",.<br />

MeR!2IurerTlPrnt point tm mountin9 Rnds Figure 7. 3-1 Defil1ition a/takil1g a Cover MC(Jsuremelll by Spot Testing<br />

The cover <strong>for</strong> possibl e new mounting rods has to be measured at<br />

least one point.


A report should be made of the cover measurements incorporating<br />

the three values obtained <strong>for</strong> the load bearing rein<strong>for</strong>cements<br />

together with the average of these. An additional report should be<br />

given <strong>for</strong> the mounting rod cover.<br />

scope<br />

General<br />

Taking measurements of the cover can be relevant in the fol lowing<br />

situations:<br />

It is likely that the cover is less than Ihal described, e.g. on the<br />

underside of the bridge deck, and areas with rein<strong>for</strong>cement guides<br />

or h a lf~ lap joints.<br />

Neither rein<strong>for</strong>cement spacers nor mounting rods have been used.<br />

Clearly corroding rein<strong>for</strong>cement with little cover ava ilable.<br />

Large amount of stress due to chloride.<br />

Places where other materials investigations are being carried out.<br />

Figure 7.3-2: Measurillg the COI'cr<br />

Acceptance Inspection<br />

The cover of all concrete elements should be checked if this has<br />

not already been done during the construction phase. For small<br />

bridges such as culverts and single-span simply supported bridges<br />

at least ten measurements should be taken of the cover spread over<br />

both Ihe super and substructures. For larger bridges the scope of<br />

testing should be evaluated, but should lie between 5 and 10 measurements<br />

per 100 square metres of concrete.<br />

Major Inspection<br />

If it is suspected that there is little cover, spot checks should be<br />

conducted of the cover. Should these suspicions be confinned,<br />

then the scope of the inspections can be extended.<br />

Special <strong>Inspections</strong><br />

Measurement of the cover is 10 be carried oul in accordance with<br />

specifi c requirements. The scope and location should be adapted<br />

to the situation.<br />

Equipment<br />

Advantages and<br />

Disadvantages<br />

* Covermeter<br />

* Drawings of the rein<strong>for</strong>cement, if necessary<br />

* Folding rule<br />

* Sl ide calliper<br />

* Chalk<br />

* Hammer aclion drill <strong>for</strong> use in measurementlesting<br />

* Materials and equipment <strong>for</strong> refilling holes<br />

This is a simple, n o n~d estructive, speedy method which allows<br />

one 10 chec k large areas in a short lime. The di sadvantage is that<br />

some cover meters indicate an incorrect cover thickness <strong>for</strong> closely<br />

spaced rein<strong>for</strong>cement. Cover meters should there<strong>for</strong>e be ca libra~<br />

ted according to the density of the rein<strong>for</strong>cement.


7.3.2 Measuring the Depth of Carbonation<br />

Purpose<br />

To measure the depth of carbonisation in concrete in order to<br />

assess the risk of corrosion of tile rein<strong>for</strong>cement or to discover the<br />

cause of the damage.<br />

Carbonisation wi ll 1ead to corrosion of the rein<strong>for</strong>cement once the<br />

carbonisation has reached the actual re in<strong>for</strong>cement elements.<br />

Carbonisation in concrete progresses most quickl y in a dry climate<br />

(inland areas) and/or in areas subject to road traffic or ind ustri al<br />

pollution.<br />

Figure 7.3-3: Carbonised COllcrete<br />

Carboni sation is nol usually a problem in good qua lity concrete<br />

and when the cover is described as being 30 mm or morc and has<br />

been so applied.<br />

Procedures<br />

Reference is made to the NOf\vegian Public Roads Administration<br />

<strong>Handbook</strong> No. 0 15: "On Site Testing", Method No. 15.554.<br />

scope<br />

General<br />

Measuring the depth o f carboni sat ion can be necessary in the fo l­<br />

lowing cases:<br />

* <strong>Bridge</strong>s built during or immedi ately after the Second World War<br />

* Older girder bridges ut ili sing unstressed rein<strong>for</strong>cement and clo<br />

sely spaced rein<strong>for</strong>cement guides on the underside of the beams;<br />

these may also have been cast in concrete without stone ele<br />

ments.<br />

* Sections with little cover (I 0-30 mm)<br />

* Sections showing clearly corroded rein<strong>for</strong>cement<br />

* Sections containing porous or bad quality cement<br />

* When cutting out pieces of concrete or making chl oride profil es<br />

Acceptance Inspection<br />

Measuring the depth of carbonisation is not necessary in this case.


Major <strong>Inspections</strong><br />

Whenever carbonisati on is suspected as a problem, spot tests<br />

should be undertaken over a sufficientl y large area so as to be abl e<br />

to conclude whether carbonisation is/is not a problem <strong>for</strong> the bridge<br />

in question. Should these suspicions be confirmed then the<br />

scope of the testing can be en larged. In add ition measurements<br />

should be taken of the cover (compare Chapter 7.3.1 <strong>for</strong> the recor·<br />

ding of the extent of the earbonisation). As an alternative a special<br />

inspection can be requisitioned.<br />

Special <strong>Inspections</strong><br />

The depth of the carbon isation is to be measured in accordance<br />

with special instructions. The extent and location should be adap·<br />

ted to during execution of the inspection.<br />

Advantages and<br />

Disadvantages<br />

Eq uipment<br />

The method is quite simple but req uires cutting or dri ll ing of the<br />

structure.<br />

• A I % solution of phenolphthalein, or possibly I gm. phenol ph<br />

tha lein in all. mixture of water (50%) and ethanol (50%).<br />

• Spray bottle<br />

• Fold ing n ile<br />

• Slidingcall iper<br />

• Hammer<br />

• Chi se l<br />

• Pure water<br />

• Material and equipment <strong>for</strong> refi lling holes<br />

• Core drilling equipment, ifnecessary<br />

7.3.3 Measuring Chloride Content<br />

Pu rpose<br />

To measure the chloride content of hardened concrete at various<br />

depths so as to evaluate the risk of corrosion of the rein<strong>for</strong>cement<br />

or 10 uncover the cause of damage.<br />

The penetration of chloride wil l cause corrosion of the re in<strong>for</strong>cement<br />

in the event of the chloride concentration becoming too hi gh.<br />

The limit <strong>for</strong> critical chloride content, namely a level wh ich can<br />

lead to corrosion of the rein<strong>for</strong>cement, was earl ier assumed to be<br />

around 0.06% of the weight of the concrete (0.4% of the weight of<br />

the cement). However, ex perience gained fro m the bridges mana·<br />

ged by the Public Roads Admini stration indicates that the chloride<br />

content can be much higher without the occurrence of damaging<br />

corrosion of the rein<strong>for</strong>cement.<br />

The following circumstances are of significance <strong>for</strong> the speed of<br />

corrosion and must be considered in conj unction with the recorded<br />

chl oride content:


* The density of the concrete in relationship to the transfer of oxy<br />

gen (quality of the concrete, thickness of the cover).<br />

* The electrochemical properties of the concrete (variation in its<br />

qual ity, high mo isture content, possible presence of macro<br />

cells).<br />

Chl oride can penetrate concrete via three different sources:<br />

* Embedded chloride<br />

* Defrosting sa lt<br />

* Mari ne climate<br />

Embedded Chloride<br />

This can be found in older bridges due to the lise of sea water<br />

during construction, or aggregate or setting agent containing chloride.<br />

The use of sea water and aggregate dredged from the sea<br />

were previously acceptable and can still be found in several older<br />

coastal bridges.<br />

Calcium chloride (CaCI) is used as a setting agent especially by<br />

the concrete casting industry to allow casts to be speedily released<br />

<strong>for</strong> reuse. Elements so cast can be found, <strong>for</strong> example, on the<br />

underside of bridge decks supported on steel plates where the brid·<br />

ge deck is partially prefabricated.<br />

Embedded chloride produces a flat chloride profile deep within<br />

concrete. The chloride profile can be overlaid by chloride which<br />

has penetrated from outside the concrete. A further effect of carbo·<br />

ni sation wi ll be a reduction in the concrete's ability to bind the<br />

chlorides. Consequently the chloride profi le achieves a low value<br />

in carbonised concrete or in crushed stone with a hi gher concentra·<br />

tion at the leading edge of the carbonisation process be<strong>for</strong>e the<br />

concentration flattens out to the embedded level. (Refer to Figure<br />

7.3-4)


Carbonation Depth<br />

OL-________ L-~~------------~<br />

o<br />

Depth<br />

'Figure 7.3-4:Chloride Pl'Oji/c.embeddefJ chlol'ide ill C(ll'bollisetl COl/crete<br />

Defrosting salt<br />

Chloride resulting from defrosting salt or sand mixed w ith salt is<br />

able to penetrate the bridge deck fro m the topside if tl1-e bridge has<br />

not been equipped with a damp course. The fo llowing ca n be considered<br />

as vulnerable areas:<br />

* Edge girders and the underside of bridge decks along a bridge's<br />

edges<br />

* Joint constructions<br />

* Pillars supporting approach sections to a bridge<br />

* Abutment piers and cul vert walls situated 0 - 2 m. from a bridge<br />

* Localised areas under water outl ets and otherwise in depressi<br />

ons where waler is stagnant .<br />

Marine Climates<br />

Vu lnerable sections of coastal concrete bridges are described in<br />

Chapter 7.3.9.<br />

Procedures<br />

Reference is made to the Norwegian Public Roads Administration<br />

<strong>Handbook</strong> No. 0 14: " Laboratory Testing" and No. 015: "On Site<br />

Testing".<br />

The diffe rences in depth of the measurements and the intervals<br />

between test sites in a profile must be estimated in light of the<br />

positioning of the rein<strong>for</strong>cement and the objective oft he test. In<br />

some cases the intelVals detai led in Procedura l Codc-2 can appear<br />

to be a little rough. The alternative depth intervals <strong>for</strong> 30 mm. and<br />

50 mm. respectively <strong>for</strong> a pl anned cover could <strong>for</strong> example be:<br />

30 mm planned cover:<br />

50 mm planned cover:<br />

2-10 mm ., 10-20 mm. , 20-30 mm., 30-45 mm., 45-70 mm.<br />

2-15 mm., IS-3D mm., 30-50 mm., 50-75 mm. , 75- 100 mm.


Any dust should be extracted using an 18 mm. dri ll from four test<br />

hol es per test. The holes should <strong>for</strong>m the corners of a 5X5 em .<br />

Square.<br />

Methods<br />

Figure 7.3-5. Drilling 0111 Cemelll<br />

Dlis/<br />

Equipment<br />

Figure 7.3-6: RCT Allalysis Case<br />

Scope<br />

The choice of method of analysing concrete dust - on site or in a<br />

laboratory - depends fi rst and <strong>for</strong>emost on how much accuracy is<br />

required and on the costs.<br />

On Site Methods<br />

The most common methods are RCT (Rapid Chloride Test) and<br />

Quantab. Reference is made to the National Public Roads<br />

Administration <strong>Handbook</strong> No. 015: "On Site Testing", Methods<br />

15.552 and 15.553. These methods are less precise than those used<br />

in a laboratory, but in most cases they will be sufficiently accurate<br />

provided they are checked aga inst reference dust or laboratol)'<br />

methods.<br />

* Equipment fo r test extrac tions (hammer effect drill)<br />

* Plastic bags fo r collecting the dust in<br />

* Felt-tip pens <strong>for</strong> marking the tests<br />

* Material and eq uipment <strong>for</strong> refi lling the holes<br />

* Equipment <strong>for</strong> analysis purposes (on site kit)<br />

* Scales with an accuracy of III 0 grams<br />

* Dust <strong>for</strong> reference purposes<br />

Laboratory Methods<br />

The most common laboratory methods are potentiometric titration<br />

and Vo lhardt's Method. Laboratory methods must be used whenever<br />

the results of the analyses have to be very precise.<br />

The analysis methods are described in the National Pub lic Roads<br />

Administration <strong>Handbook</strong> No. 014: "Laboratory Testing", whil st<br />

Volhardt's Method is described in NS 3671.<br />

Acceptance Inspection<br />

So far as large new coastal bridges are concerned routines require<br />

to be established in connection with taking chloride measurements<br />

from selected construction elements. Any incursions of chl oride<br />

should be followed up with repeated measurements during future<br />

main inspections.<br />

Otherwise, measurements of the chl oride content are not taken<br />

during completion inspections.<br />

Major <strong>Inspections</strong><br />

If embedded chloride is suspected, <strong>for</strong> example, because of the<br />

visible results of corrosion, peeling and corroded rein<strong>for</strong>cement on<br />

the surface concrete, measurements should be taken of the chloride<br />

content.


For roads subject to salti ng spot checks of the chloride content<br />

should be taken in exposed areas such as pi llars supporting the<br />

approach sections to a bridge and the edge girders of bridges along<br />

the route. This is most va lid <strong>for</strong> bridges constructed according to<br />

older regulations, namely be<strong>for</strong>e 1996/97.<br />

Repeated chloride content measurements ought to be taken during<br />

each main inspection at approximately the same locations as a fol ­<br />

low-up over time. Measures can accordingly be taken timeously<br />

should the need arise.<br />

For new large coastal bridges inspection routines should be fo llowed<br />

or establi shed if necessary.<br />

Spot tests should be carried out on older bridges which have not<br />

previously been chec ked <strong>for</strong> chloride incursion. The need <strong>for</strong> a<br />

special inspection incorporating more extensive materials tests<br />

should be assessed.<br />

Measurements of the covering and the depth of any carbonisation<br />

should be undertaken at the sa me time as any dri lling <strong>for</strong> dust in<br />

connection with chloride tests. Alternatively a special inspection<br />

can be carri ed out including comprehensive materials testing and,<br />

if necessary, EC P measurements.<br />

Special <strong>Inspections</strong><br />

Chloride measurements are carri ed out according to special prescriptions.<br />

Their extent and location should be taken into during<br />

execution of the test.<br />

Ad vantages and<br />

Disadvantages<br />

On site testing is cheap and easy to carry Oul but are less accurate<br />

than laboratory methods. Analyses conducted in a laboratory are<br />

time-consuming and costly but result in a high level of accurac<br />

7.3.4 Corrosion Testing (ECP)<br />

To measure the rein<strong>for</strong>cement's electrochemical potential (ECP)<br />

and associated resistance in order to assess the probability of the<br />

rein<strong>for</strong>cement co rroding.<br />

Procedures<br />

Reference is made to the National Publ ic Roads Administration<br />

<strong>Handbook</strong> No. 0 15: "On Site Testing", Method NO. 15.552 and the<br />

National Pub lic Roads Administration, <strong>Bridge</strong> Division's Report<br />

No. 94- 16 <strong>Bridge</strong>s:<br />

"Recommendations <strong>for</strong> the Equipment <strong>for</strong> Measuring<br />

Electrochemical Potential (ECP)".<br />

General<br />

Scope<br />

ECP measurements should be taken if latent rein <strong>for</strong>cement corrosion<br />

is suspected.


Completion Surveys & Major <strong>Inspections</strong><br />

ECP measurements are not normally taken in these instances. The<br />

need <strong>for</strong> such tests during a main inspection will be init iallyassessed<br />

on the basis of visual observati ons and the resul ts of the tests<br />

both of the depth of carbonisation and the chloride c ontent.<br />

Special <strong>Inspections</strong><br />

EC P measurements should be conducted as per special instructions<br />

and should be verified by cutti ng into the concrete. Refer to<br />

Chapter 7.3.8. The chloride content, depth of carbonising and<br />

cover should all be measured at the place where the concrete is cut<br />

inlo.<br />

Advantages and<br />

Disadvantages<br />

•<br />

FigWl? 7.3-7: Takil/g ECP<br />

AI eusu rem e illS<br />

Equipment<br />

Figure 7.3-8: Drillil/g Ollt (I<br />

Concrete Core<br />

Methods<br />

This method is easy to use, non-destructive and rel"tively quick<br />

with the resu lt that large secti ons can be checked. It can provide a<br />

satisfactory picture of the cond ition of the rein<strong>for</strong>ce ment at any<br />

given moment. The risk of corrosion can be detectetd during an<br />

earl ier phase be<strong>for</strong>e visible damage becomes obvious. People possessing<br />

professional competence should be used both <strong>for</strong> site work<br />

and the interpretation of the results. The method does not record<br />

the speed of the corrosion process.<br />

ECP Equipment:<br />

• Metering electrodes<br />

• Voltmeter<br />

• Cables<br />

• Data recorder<br />

Other:<br />

• Spray bottle <strong>for</strong> moistening concrete<br />

• Device <strong>for</strong> measuring the cover<br />

• Clips <strong>for</strong> mak ing contact wilh the rein<strong>for</strong>cement<br />

• Chalk<br />

• Wire brush<br />

7.3.5 Determining the level of Strength<br />

To detennine the compressive strength of hardened concrete<br />

should, <strong>for</strong> example, below standard concrete be suspected.<br />

Compressive strength can be determined by, amongst other things:<br />

• Pressure testing of concrete cores dri lled out<br />

• Jackhammer<br />

Pressure testing of concrete cores drilled 0 ut<br />

Procedures<br />

Advantages and<br />

Di sadvantages<br />

Reference is made to the Norwegian Public Roads Admini stration<br />

<strong>Handbook</strong> No. 015: "On Site Testing" <strong>for</strong> the drilliog Oul of concrete<br />

cores, and to the Nat ional Public Roads Administration<br />

<strong>Handbook</strong> No. 014: " Laboratory Test ing" fo r pressure testing the<br />

concrete cores.<br />

This methods produces precise pressure test val ues <strong>for</strong> the cores in<br />

question, but does req uire expensive equipment and is to be consi-


dered time consuming. This is a destructive method; one has to<br />

take care du ring the dri ll ing process so as to avoid damaging the<br />

rein<strong>for</strong>cement. Core dril ling in pre-stressed concrete bridge elements<br />

should be carried out only in special situations.<br />

Equipment<br />

* Core drilling equipment<br />

* Materials and equipment fo r refilling the hol es<br />

* Pressure testing device<br />

Rebound Hammer<br />

Procedures<br />

Reference is made to the Norwegian Public Roads Administration<br />

<strong>Handbook</strong> No. 0 15: "On Site Testing", Method No. 15.544.<br />

Figure 7,3-9: Measurillg the<br />

Compressive Strength o/ Col/crete<br />

!lsillg a Rebowui flammer<br />

Equipment<br />

This is an extremely speedy, simple and cheap method. However,<br />

the test results are very inaccurate because of a great deal ofuncertainty<br />

about them. Nevertheless the results can be used to obtain a<br />

picture of how the compressive strength can vary in different ele-.<br />

ments. Values can be obtained only <strong>for</strong> a concrete surface.<br />

* Schmidt hammer or pendulum hammer<br />

General<br />

Scope<br />

The strength level of concrete is rarely lower than that used as a<br />

basis at the design stage. Generally speaking the need <strong>for</strong> compressive<br />

strength testi ng does not arise during routine inspections.<br />

Acceptance <strong>Inspections</strong> and Major <strong>Inspections</strong><br />

Determining compressive strength is not usual ly carried out.<br />

Special <strong>Inspections</strong><br />

Determining compressive strength may be necessary should the<br />

load bearing capacity be too low, and verification of the actual<br />

strength can benefit the calculati ons.<br />

Purpose<br />

Procedures<br />

7.3.6 Structural Analysis<br />

To determine the structure of the concrete by analysi ng the results<br />

of Plane Ractify ing and/or of Thin Section Method to discover<br />

amongst other things the reason <strong>for</strong> any damage, e.g. alka li reactive<br />

aggregate.<br />

Concrete structures will be analysed using surface gri nding or fine<br />

grinding depending on the purpose of the analysis. Both types of<br />

anal ysis are carried out in a laboratory on drilled out cores.<br />

Plane Ractifying<br />

A concrete core is sawn along its central axis, burnished and surface<br />

treated. Surface grinding providcs the following in<strong>for</strong>mation:<br />

* The \VIc ratio


• Homogeneity of the binding agent<br />

* Distribu tion of the aggregate (quality)<br />

• Air content Idi stance between air bobbles? (durabil ity aga inst<br />

frost)<br />

• Cracking<br />

Thin Section Analysis<br />

A piece of fin e ground concrete nonnally measures 40 x 45 mm.<br />

and is ground down to a th ickness of20-25 my. Apart from that<br />

obtained from surface grinding, fin e grinding provides the fo llowing<br />

addit ional in<strong>for</strong>mation:<br />

• Carbonisation<br />

• Leve l of hydration (q ualitative)<br />

* Type of aggregate<br />

• Chemical reactions such as reaction to alkali<br />

Scope<br />

Acceptance <strong>Inspections</strong> and Major <strong>Inspections</strong><br />

Structural analyses sha ll not be carried.<br />

Speciallnpections<br />

Structural analyses are carried out only when required, e.g. suspected<br />

reaction to alkali.<br />

Advantages and<br />

Disadvantages<br />

Plane Ract ifying and th in section analysis are both good methods<br />

<strong>for</strong> detennining concrete qua lity but are destructive, costly and<br />

time consuming. They should only be considered if the possible<br />

damage and its causes cannot be detennined using any other method<br />

or when it is important to know the composition of the concrete.<br />

Since only a small part of a structure is examined, it is vital that<br />

representative dri ll ed cores are removed <strong>for</strong> analysis and that<br />

wide-ranging conclusions arc not drawn from the analysis resu lts.<br />

Figure 7.3-10: Analysis IIsing Thin Sec/ioll Me/hod<br />

Equipment<br />

• Core drilling equipment<br />

• Laboratory analysis equipment


Purpose<br />

Procedures<br />

7.3.7 Inspection of Prestressed Tendons<br />

To conduct an inspection of the condition of pre-tensioned and<br />

post-tensioned cabl es anchored in concrete. Checking pre-tensioned<br />

cables may be worthwhile if defective injection is suspected,<br />

as this can have very serious consequences <strong>for</strong> the bridge's load<br />

bearing capacity.<br />

Checking post-tensioned cables is difficu lt and should only be carried<br />

out by a specialist company using special equipment, and then<br />

only after consulting the bridge's designers.<br />

Ultrasound, X-rays or a fibre optic endoscope can be used to locate<br />

damage. The use of a fibre optic endoscope requires holes to be<br />

drilled in the cable tubes. One should, there<strong>for</strong>e, have a clear<br />

understanding of where the cavities and the damage arc located, as<br />

drilling incorrectly and damaging a tension cabl e can have serious<br />

consequences.<br />

Scope<br />

Acceptance <strong>Inspections</strong> and Major <strong>Inspections</strong><br />

Tension cables are not normally checked.<br />

Special <strong>Inspections</strong><br />

A tension cable check wi ll be undertaken as required, fo r example<br />

when badly executed injection of the cable tubes is suspected.<br />

Fig1lrc 7.3-/1<br />

Fib.·c Optic Testiflg<br />

of a Tel/siollcd Cable<br />

Advantages and<br />

Disadvantages<br />

Equipment<br />

Purpose<br />

A good overview can be obtained of the conditions inside a cable<br />

tube, but the method is destructive and it is all too easy to hit the<br />

cable tube or the cavit ies. In addition there is a risk of damaging<br />

the cable itself.<br />

To be decided <strong>for</strong> each specific occasion.<br />

7.3.8 Cutting open the Concrete to Assess the<br />

Corrosion level<br />

To carry out a visual check of the level of corrosion in the rein<strong>for</strong>cement<br />

and to record the type of rein<strong>for</strong>cement and its diameter.<br />

Additional ly, the cover should be measured.


Procedures<br />

In most cases it is sufficient <strong>for</strong> the width of the area to be cut to<br />

match the dimensions of the re in<strong>for</strong>cement and the cover sllch that<br />

the minimum width equals the cover plus the diameter of the rein<strong>for</strong>cement<br />

(0 + d). Refer to Figure 7.3- 12. Approximately 1/3 to Y2<br />

of the rein<strong>for</strong>cement element's circumference s hou~d be bared <strong>for</strong><br />

atleasl 0.3 cm.<br />

.r<br />

minimum<br />

O+d<br />

.r<br />

.-<br />

:T-<br />

O<br />

:Ty<br />

d r<br />

Figllre 7.3-/2: Recommended Breadll! & Deplh oflhe CIIII/llc ision<br />

The degree of rusting in the rein<strong>for</strong>cement wi ll be assessed usi ng<br />

the fo llowing scale:<br />

Level A: No damage. Dull grey coating on the rein <strong>for</strong>cement ele<br />

ment.<br />

Level B: The first small traces ofrus! can be seen. Assess whether<br />

these date from the bridge's construction period.<br />

Level C: Even distribution of surface rust.<br />

Level D: Severely peeling surface rust as we ll as clear cross-secti<br />

onal reduction in size.<br />

Level E: Corrosive pi tting.<br />

The degrees of rust ing are illustrated in Figures 7.3-13 to 7.3-17.<br />

Figllre 7.3-/3: Example ofRusl Level A


Figl/Ye 7.3-14: Example 0/ Rilsi lel'ef B<br />

Figllre 7.3-15: £wmp/e 0/ RIiSf Lel'ef C<br />

Figllre 7.3-16: bump/eo/Rllsf Lel,e/ D


Figure 7.3-17 E.wmpleQJRlIsl Level £<br />

Cutting open the concrete reveals the actual level of corrosion to<br />

the rein<strong>for</strong>cement and acts as a check <strong>for</strong> the resu lts of other materials<br />

testing. The method is destructive and ought only to be<br />

employed to a very limited ex tent. It shoul d be noted that the area<br />

to be cut open is not necessarily representative of an entire bridge.<br />

Acceptance <strong>Inspections</strong> & Major <strong>Inspections</strong><br />

Cutting open concrete fo r corrosion assessment purposes is not<br />

usually undertaken. However, it can be worthwhi le in the assessment<br />

of any cross-secti onal reduction in the rein<strong>for</strong>cement when<br />

there is visible evidence of corrosion.<br />

Special <strong>Inspections</strong><br />

tain ing latent corrosion. In these cases areas with cl ear evidence of<br />

corrosion should not be cut open.<br />

Should noth ing else specifica lly be mentioned, then cutting operations<br />

should be undertaken <strong>for</strong> consecutive areas measured <strong>for</strong><br />

potentiality <strong>for</strong> the following locations:<br />

* The lowest measure of potentiality<br />

* The middle measure of potentiality<br />

* The highest measure of potentiality<br />

When cutting into concrete to veri fy ECP measurements the fo llowing<br />

materials tests should be undertaken in the order given:<br />

I. ECP measurements (recording the potential and resistance<br />

levels)<br />

2. Measuring concrete cover<br />

3. Measurin g the ch loride content from layers adj usted <strong>for</strong> the<br />

cover measured such that the chloride level is measured in each<br />

or the layers.<br />

4. Cutting operati ons and evaluating the level o f rust and the<br />

reduct ion in the cross-section.<br />

5. Measuring the depth of ca rbonisation


6. Measuring the actual cover to check the cover meter<br />

7. Re-filling<br />

Cutting into concrete can also be carried out in connection with the<br />

assessment of the scope of corrosion to the rei n<strong>for</strong>cement elements.<br />

Barriers should also be cut open to assess the reduction in<br />

cross-sectional reduction of the rein<strong>for</strong>cement. Areas showing<br />

visible signs of surface corrosion of the concrete should be approached<br />

in a similar fashion. This is especiall y desirable <strong>for</strong><br />

barrierslthe results of corrosion which are found in areas prone to<br />

static strain.<br />

Equipment<br />

* Cutting equipment (chisel hammer)<br />

* Camera<br />

* Slidc callipcr<br />

* Magnifying glass<br />

* Wire brush<br />

* Materials and equipment <strong>for</strong> refilling holes<br />

7.3.9 Location of Materials Testing <strong>for</strong><br />

Concrete Coastal <strong>Bridge</strong>s<br />

Chloride Penetration<br />

It has become apparent that chloride penetration on exposed coastal<br />

bridges is characterised principal ly by three sets of circumstances:<br />

I. Height above Sea Level: Chloride penetration increases<br />

according to the he igh t of the superstructure above sea level ­<br />

refer to Figures 7.3- 18 and 7.3- 19. The same applies to co lumns<br />

(see Figure 7.3-20). However, in some instances the chloride<br />

contem has been shown to be lower further down the columns<br />

than nearer the top.<br />

2. The Windward/Leeward Effect: Chl oride penetration is mar<br />

kely greater on surfaces subject to wind and rainfa ll on the lee<br />

ward side. The effects can depend on their being/not being sub<br />

ject to rain and negative pressure on the leeward side resu lting<br />

in sea spray settling on the concrete surfaces - refer to Figures<br />

7.3-18and 7.3-19.<br />

Leeward facing surfaces are to be found on both the sub and superstructures.<br />

The following are some typ ical examples:<br />

* Vertical surfaces in the lee of wi nd and ra infall (columns, webs<br />

in box gi rders and beams.<br />

* Horizo ntal downward fac ing surfaces - the undemeath of top<br />

cross-beams, beams, top plates and wings, and base plates of<br />

box girder bridges.


"<br />

~<br />

~<br />

~<br />

•<br />

E<br />

E<br />

u<br />

B<br />

~<br />

~<br />

u<br />

'"<br />

~<br />

0<br />

•<br />

...<br />

0<br />

-.<br />

g~<br />

";: ...J<br />

<br />

"Qj ..8<br />

~ .<br />

~<br />

,.<br />

'"<br />

'.<br />

,. .'<br />

~<br />

... .. .. ,.. "<br />

-<br />

~<br />

~ 'OO<br />

;" . .<br />

.. -<br />

~\..-~,,'"'<br />

.'<br />

,<br />

,<br />

,<br />

, ..<br />

'"<br />

.. , . •<br />

CD ,<br />

BeJow Bo~ Girder<br />

."~ Wall<br />

..........<br />

Figure 7.3-18: Average Chloride Content in the Box Girders. Gimsoyslruwllen<br />

<strong>Bridge</strong>al a Depth 0[0- /0 mm.<br />

""""\<br />

=:c..::::::::c=<br />

-'---- --o:c;;::::::::=<br />

"~[ ~KS! ~ . 1'1.11'<br />

____ I.. South O))'lIO ~ ':;<br />

Dominant Wind<br />

DirectiOf1 during<br />

Precipitation 022'11. s'7 6<br />

--''---~-+<br />

North<br />

.-<br />

ktr116<br />

1<br />

::--:-_.".~ South 0119'1'­<br />

Dominant Wind<br />

Direction during<br />

Presipilalion<br />

North<br />

::--,.-,,,,,I~ South<br />

Dominant Wind<br />

Direction during<br />

Precipitation<br />

Ao(SE<br />

'] • 74m •<br />

"<br />

"<br />

'66%<br />

North<br />

Chloride conlent as % of cement weight <strong>for</strong> depths (}'1 0 mm<br />

Figure 7.3- 19: Varia/ioll a/Chloride Con/enl of Box Girders according to<br />

Height above Sell-fel'el.


t I e<br />

---::--._.- . -.<br />

._'_.. !<br />

Figure 7.1-10: V(lrimioll ill Chloride COl1lel1l OfCO/III11I1S accQrding 10 Height<br />

above Sea-/e~·e1-Gil/lsoystraulllen <strong>Bridge</strong><br />

3. Geometric Effects: Exposure is greater on large cross-sections<br />

and badly geometrically shaped cross-sections - see Figure 7.3-<br />

18.<br />

In addition, local circumstances can exist related to the terrain<br />

around the bridge or to the sea bed around the columns and which<br />

can also affect chloride impact (skerries and foundations produce a<br />

lot of spray).<br />

All of these factors produce simultaneous effects and a joint chloride<br />

impact pattern.<br />

The following contains a rough overview of those sub and superstructural<br />

surfaces most and least exposed to chlorides.<br />

Surfaces most exposed<br />

to Chloride Penetration<br />

Surfaces least exposed<br />

to Ch loride Penetration<br />

Substructure<br />

Large cross-sections of the leeward side of columns between 0 and<br />

20 metres above the surface oflhc water, e.g. the ma in columns of<br />

cantilever bridges; also the underneath of top cross-beams near the<br />

surface of the water.<br />

The windward sides of thin columns with a high elevation above<br />

sea-level.


Superstructure<br />

Surfaces most exposed<br />

t o Chloride Penetration<br />

Surfaces least exposed<br />

to Chloride Pene tratio n<br />

Chloride and Mo isture<br />

Combination of<br />

Materia ls Testing<br />

Leeward facing surfaces low down and near the water surface,<br />

especially large cross·sections, <strong>for</strong> example pil lars of Cantil ever<br />

<strong>Bridge</strong>s;also the underneath of bottom plates, cross girders and<br />

beams.<br />

The windward sides of sl im superstructures with a hi gh elevation<br />

above sea· level.<br />

Concrete surfaces containing a high level of chloride will retain<br />

moisture longer during the drying out process and will consequently<br />

be of a darker shade than surfaces with a low salt content.<br />

It is there<strong>for</strong>e possible in a damp coastal cl imate to see with the<br />

naked eye which surfaces have most been affected by chloride.<br />

Surfaces greatly subject to wind and rain (on the windward side)<br />

will gradually acquire a sandy appearance because the top surface<br />

layer of the concrete will have been washed away.<br />

When deciding the places to undertake materials testing one<br />

should make use of this knowledge of chloride instigated stress.<br />

It is important to carry out several kinds of materials testing, e.g.<br />

surface cover measurements, chloride analyses, ECP measurements,<br />

cutting open the concrete, in such a way that these can be<br />

compared wi th one another be<strong>for</strong>e the condition of the concrete is<br />

decided on. Materials testing should also be viewed in relationship<br />

to any visual inspections undertaken.<br />

in order 10 be able to compare the result's of materials testing such<br />

as surface cover and ECP measurements, measuring the chloride<br />

content and the depth of carbonisation, and cutting open the concrete,<br />

they must all be carried out at the same places. Refer to<br />

Chapter 8.5 <strong>for</strong> a presentation of materials testing <strong>for</strong> concrete.<br />

7.4 Adequate Materials<br />

Testing - Steel<br />

In the following section a description wi ll be given of the possible<br />

materials testing <strong>for</strong> use in inspections of bridge sib ridge elements<br />

made of steel.<br />

Purpose<br />

Procedures<br />

7.4.1 Checking the Torque of Screws<br />

To check the stud torque of screws in friction joints.<br />

Checking the torque of screws may be necessary in connection<br />

with acceptance inspections if this has not already been carried out<br />

during the construction phase. Reference is made to the National<br />

Public Roads Admini stration Manual No. ISO: '<strong>Bridge</strong>s - Safety<br />

and Technical Standards', Point NO.7.


This check may also prove necessary during Special <strong>Inspections</strong><br />

should there be any suspicion of screws having lost theirorigina l<br />

tension.<br />

Equipment<br />

• Torque wrench<br />

Purpose<br />

Procedures<br />

Equipment<br />

7.4.2 Checking Rivets and Screws<br />

To check whether rivets and/or screws are loose or have possibly<br />

dropped out of place.<br />

Loose screws or ri vets can cause cracks to appear in the surface<br />

treatment at the cross-over point between screw/rivet head and the<br />

basic material. By lightl y tapping on one side oflherivet wi th a<br />

hammer whi le placing one's finger on the opposite side of the ri vet<br />

at the cross-over point one can feel whether the ri vet is loose.<br />

• Magnifying glass<br />

• Torch<br />

• Hammer<br />

Figure 7.4-/: Checking a RiI'el<br />

Equipment<br />

Purpose<br />

Procedures<br />

Equi pment/Competence<br />

7.4.3 Checking Welds<br />

To carry out visual check <strong>for</strong> fau lts in the welding or whether<br />

damage has been caused to the welding.<br />

If material defects are suspected, X-ray or ultrasound checks<br />

should be carried out in addition - see points 7.4.4 and 7.4.5.<br />

• Magni fy ingglass<br />

• Torch<br />

• Tool <strong>for</strong> measuring the width of cracks<br />

7.4.4 X-ray Check<br />

To carry out X-ray inspections of welds and other steel elements to<br />

check <strong>for</strong> material defects.<br />

The X-ray fi lm should be used to document the results.<br />

The inspection should be undertaken by a pe rson with the relevant<br />

training and the necessary speciali st equipment.<br />

Purpose<br />

Procedures<br />

7.4.5 Ultrasound Check<br />

To ascertain with the use of ultrasound equipment whether there<br />

are material defects in welds, or cracks in screws or ri vets.<br />

Reference is made to Procedure No. 87. 1835<br />

The measurements should be taken using a test sensor whi ch transmits<br />

and receives ultrasound waves which actually work on a frequency<br />

beyond the that of human hearing (approx. 16,000 Hz).


The sound waves can be transmitted into solid materials, but not<br />

air. The test sensor should be placed on the surface; the sound<br />

waves are then bounced off the reverse surface oflhe test area.<br />

The results are recorded via an oscilloscope, and their interpretation<br />

places great demands on the operator. This person should possess<br />

the necessary qualifications and ex perience <strong>for</strong> recording and<br />

interpreting the results.<br />

X-ray and ultrasound tests complement each other. Ultrasound testing<br />

is the preferred method <strong>for</strong> checking <strong>for</strong> faults in bonding<br />

materials and certain types of cracks.<br />

Eq u i p me ntl Com pete nce<br />

Purpose<br />

Procedures<br />

Purpose<br />

Procedures<br />

E qu i p mentl Com petence<br />

These checks should be carried out by companies with properly<br />

trained personnel and special equipment.<br />

7.4.6 Magnetic Powder Check<br />

To check <strong>for</strong> the presence of cracks in the steel which are not<br />

visibl e to the naked eye.<br />

The extent of the cracks should be documented by means of drawings<br />

or photographs. Both cracks all the way through the steel<br />

and on the surface are to be drawn as a record. This type of test<br />

does not provide any measurements of the depth of the cracks.<br />

These checks should be carried out by companies with properly<br />

trained personnel and special equipment.<br />

7.4.7 Fi bre Optics<br />

To check <strong>for</strong> the presence of damage, e.g. corrosion or cracks, in<br />

enclosed or not easily accessible steel elements with the use of a<br />

fibre-optic equipped endoscope.<br />

These checks should be carried out by companies with properly<br />

trained personnel and special equipment .<br />

Purpose<br />

Procedures<br />

Eq u i p m e ntl Com pete nce<br />

7.4.8 Ultrasound Measurement of Material<br />

Thickness<br />

To measure the thickness of steel parts when directl y taken measurements<br />

are not possible, <strong>for</strong> example when only one of the steel<br />

surfaces is accessible. This may be the case with corrugated steel<br />

pipes and piles.<br />

Reference is made to Procedure 87.1838 and Chapter 7 A.5. The<br />

possibl e results of corrosion on the reverse surface do not reflect<br />

ultrasound impulses. The effecti ve thickness wi ll there<strong>for</strong>e be<br />

measured.<br />

These checks should be carried out by companies with properly<br />

trained personnel and special equipment.


7.5 Adequate Materials<br />

Investigation - Timber<br />

This chapter contains in <strong>for</strong>mation about materials investigations<br />

which can be recommended <strong>for</strong> Ihe inspection of timb er bridges<br />

and bridge elements.<br />

Figure 7. 5-/: Measurillg Mois/ure<br />

Le l'e/s in Wood<br />

Purpose<br />

7.5.1 Investigation of the Humidity Level of<br />

Timber<br />

To measure the moisture content of timber elements. The moisture<br />

level recorded wi ll reveal, amongst other things, whether there is a<br />

danger of the existence of dry rot fun gus. This test will, however,<br />

be of usc only in special cases and only <strong>for</strong> load-bearing clements<br />

since an already high moisture level must be taken into account in<br />

limber bridges .<br />

• Electric moisture meter<br />

• Measurement electrodes<br />

Purpose<br />

7.5.2 Checking <strong>for</strong> Fungus and Rot - Timber<br />

To carry out analyses of timber in order 10 ascertain the type of<br />

fun gus wh ich has ca used the rot damage. These are worth consideri<br />

ng when the test area is large and any possible replacement of<br />

sections could have serious consequences.<br />

Procedures<br />

Equ ipment/Com petence<br />

Samples should be taken of any fungus visible and these are to be<br />

sent 10 a laboratory which conducts tests on fung i.<br />

A pi ece of wood core can also be extracted using a drill to obtain a<br />

picture of the timber's cross-section. The core removed should be<br />

of the smallest possible diameter so as to avoid weakelling the<br />

cross-section. The hole should be re-fi lled.<br />

Samples should be removed with a knife or other equipment <strong>for</strong><br />

drill ing out core sections. The analyses should be conducted by a<br />

specially equipped laboratory with com petent personnel.<br />

7.6 Adequate Materials<br />

Investigation - Stone<br />

In the fo llowing secti on a description is provided ofth e materials<br />

testing which can be used during inspections of stone bridges and<br />

bridge clements.<br />

Purpose<br />

7.6.1 Compressive Strength <strong>for</strong> Stone<br />

To ascertain the compressive strength of stone by press ure testing.<br />

This may be necessary when checking the load bearing capacity of<br />

slone bridges.


Procedures<br />

The compress ive strength of stone is ascertained by removing<br />

stone cores and subjecting these to pressure testi ng. Only stone<br />

which is representative and free from cracks and scratches should<br />

be used in core sampling. This method can also be em ployed to<br />

determine the modulus of elasticity of the stone.<br />

These tests should be carried out by suitably qualified people<br />

using specialist equipment and can be used during Special<br />

inspections.<br />

Equ ipme nt<br />

'" Core drilling equipment<br />

'" Pressure testing machine<br />

7.7 Adequate Checking of the<br />

Surface Treatment<br />

What fo llows is a description of the tests which can be carried out<br />

when inspecting the surface coating of concrete, steel or timber.<br />

These tests should primari ly used during Acceptance <strong>Inspections</strong><br />

in the absence of any records indi cating they have al ready been<br />

conducted. Moreover, they should be executed during Special<br />

<strong>Inspections</strong>.<br />

A licensed Inspector should preferably be employed <strong>for</strong> special<br />

checks of the surface coating of steel, especially when extensive<br />

maintenance work is under consideration.<br />

Purpose<br />

Procedures<br />

Equipment<br />

7.7.1 Thickness of Surface Coating -Concrete<br />

To check that the thickness of the surface coating of the concrete is<br />

as prev iously described.<br />

The test can be conducted on already cut out sections whose thickness<br />

can be directly measured by use of, <strong>for</strong> example, an instrument<br />

ror measuring the width of cracks or a magni fying glass.<br />

Alternatively <strong>for</strong> concrete a sli ver of tile surface coating can be<br />

tested <strong>for</strong> thickness.<br />

'" Core drill ing equipment<br />

'" Measuring Gauge or a Magnify ing Glass<br />

Purpose<br />

7.7.2 Adhesive Bonding between Surface<br />

Coating and Concrete<br />

To measure the surface coating's bonding to the concrete using a<br />

stripping instrument.<br />

Reference is made to the Norwegian Public Roads Administration<br />

Manual No. 0 15: 'On Site Testing' ~ Method No. 15.541 .


Procedures<br />

Equipment<br />

Surface sections subjected to stripping shoul d be treated with a<br />

new coating.<br />

Equipment:<br />

'" Stripping equipment<br />

'" Sa mpl e bea kers<br />

'" Core drill<br />

'" Quick-sett ing gl ue<br />

'" Wire brush or ordinary brush<br />

Figure 7.7-1: Strippil1g Il1sll"IImellt<br />

Purpose<br />

Procedures<br />

Equipme nt<br />

7.7.3 Depth of Penetration of Water Repellent<br />

Impregnation<br />

To measure the depth of the penetration of water repeDent impregnation<br />

in concrete.<br />

The depth of penetration is measured by cutting out sa mple cores<br />

of a minimum diameter or60 mm, cutting them open, drying them<br />

at a temperature of 50 0 - 60 0 C and using water as an indicator. A<br />

test consists o f 3 cores, and the penetration depth is recorded <strong>for</strong><br />

each of the 6 half cores using a magnifying glass <strong>for</strong> cracks.<br />

'" Core drill<br />

'" Measuring Gauge<br />

Purpose<br />

Procedures<br />

Equipme nt<br />

7.7.4 Thickness of Surface Coating of Steel<br />

To chec k that the thi ckness of the dri ed coating of paint or surface<br />

coating of steel is as previously described.<br />

Reference is made to the Norwegian Public Roads Admin istration<br />

Report No. 94-08 (<strong>Bridge</strong>s): ' Maintenance of Anti-Co rrosion<br />

Coatings <strong>for</strong> <strong>Bridge</strong>s'<br />

For Acceptance <strong>Inspections</strong> testing the thickness orthe surface<br />

coating should be carried out in accordance with the Norwegian<br />

Public Roads Administration Manual No. 150: ' <strong>Bridge</strong>s - Safe ty<br />

and Techni cal Standards', Point NO.7 if this has not been done<br />

during the construction phase. Moreover, thi s test is suited to<br />

Special In spec tions.<br />

'" Electromagneti c thickness gauge<br />

'" Feeler gauge <strong>for</strong> ca libration purposes


Figllre 7.7-2: Thicklless ofSllrface Coalingo/Sleel<br />

7.7.5 Adhesive Bonding between Surface<br />

Coating and Steel<br />

Purpose<br />

Procedures<br />

Equipment<br />

To measure the surface coating's adhesive bonding to the steel<br />

using a stripping instrument.<br />

For Acceptance <strong>Inspections</strong> measuring the surface coating's adhesive<br />

bonding should be carried out in accordance with the<br />

Norwegian Public Roads Administration Manual No. 150:<br />

' <strong>Bridge</strong>s - Safety and Technical Standards', Point No.7 if thi s has<br />

not been done during the construction phase. Moreover, this test is<br />

su ited to Special <strong>Inspections</strong>.<br />

The method is destructive and should not be used unnecessarily.<br />

Surface sections subjected to stripping should be treated with a<br />

new coating.<br />

'" Stripping instrument<br />

'" Round sheets of aluminium<br />

'" Magnet<br />

'" Quick-setting glue<br />

'" Sand paper<br />

'" Knife or simi lar 1001<br />

7.7.6 Other Checks - Surface Coating of Steel<br />

In addition to a visual check of the old surface coating <strong>for</strong> damage,<br />

the following checks may be worthwh il e in connection with<br />

Special <strong>Inspections</strong> be<strong>for</strong>e undertaking painting as part of the<br />

maintenance programme:<br />

Sectional Measurements<br />

lattice Section<br />

The thickness of the each layer of paint is measured as well as the<br />

number of coats and the th ickness of each coat (this presupposes<br />

the use of a different colour <strong>for</strong> each layer).<br />

This provides a measurement of the adhesive bonding to the bottom<br />

surface. This technique cannot be used on thermally applied<br />

coatings


Ability to Accept New<br />

Layers of Pa int<br />

Ana lysis o f o ld Pa int<br />

This should be checked with regard to old surface coatings and to<br />

the adhesive bond ing between old and new surface coatings.<br />

It can be advisable to anal yse samples of the old surface coatin g to<br />

ascertain its composition with some certainty.<br />

7.8 Readings from<br />

Instruments<br />

Instruments can be mounted on a bridge to follow the development<br />

ofa situation over a peri od of time. This will act as a suppl ement<br />

to visual checks, measurements and materials testi ng. In some<br />

instances instruments are installed to veri fy the stress levels 10<br />

which the bridge is subjected. The fo llowing are representati ve of<br />

the instruments which could be used:<br />

Instrume ntation<br />

* Reference electrodes<br />

* Equipment <strong>for</strong> measuri ng the speed of corrosion<br />

* Wind speed detector<br />

* Wave height detector<br />

* Resistant Wire Strain Gauge (on steel)<br />

* Vibrating Wire Strain Gauge (on concrete)<br />

The instruments can be read during main or special inspecti ons or<br />

separately if desired.


8 Reporting<br />

the Results of<br />

<strong>Inspections</strong><br />

8.1 Acceptance <strong>Inspections</strong> -<br />

Warranty <strong>Inspections</strong><br />

Acceptance <strong>Inspections</strong> and Warranty <strong>Inspections</strong> should preferably<br />

be printed on <strong>Bridge</strong> Management Systems inspection <strong>for</strong>ms,<br />

since these have been designed to suit each individual bridge<br />

depending on the data in the BMS module <strong>for</strong> the structure.<br />

Irthe data <strong>for</strong> some bridges have not been recorded in the BMS,<br />

indi vidual reports require to be drawn lip, the contents of which<br />

can have the fo llowing stmcture:<br />

1. Summary containing an overview of any damage, faults or<br />

defects to be repaired.<br />

2. Description of the bridge and the system afloealing damage.<br />

3. Results of visual inspections.<br />

4. Results of the measurements and material testing.<br />

5. Assessment of the recorded damage, faults or defects. Indicate<br />

which of these require repair and whether some of them may be<br />

possible sources of future destructi ve developments.<br />

8.2 Routine <strong>Inspections</strong><br />

The reports <strong>for</strong> all Routine <strong>Inspections</strong> should be printed on the BMS<br />

inspections fonns which have been designed to suit each individual<br />

bridge and type of in spection.<br />

The inspection fonns should be taken to inspections and then completed<br />

on site. The fo llowing routines can be of assistance.<br />

General <strong>Inspections</strong> require points I to 6 and 12 to be carried out.<br />

I. The Inspector should check whether there are missing or incom<br />

plete data with reference to bridge category, its position, type of<br />

stmcture or the equipment required to gain access.<br />

2. The name (initials) of the Inspector together with the date of the<br />

inspection should be completed on the <strong>for</strong>m.<br />

3. The Inspector can record any general comments about the<br />

inspection.<br />

4. Experiences, events, specific damage or the such like can be<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 117


ecorded under their own points should they be considered<br />

important <strong>for</strong> others in the future.<br />

5, Only those elements wh ich wi ll be checked during the actual<br />

inspection are to be mentioned on the inspection fonn. Elements<br />

located above the water level wi ll not be included in inspection<br />

fonns used <strong>for</strong> Ma in <strong>Inspections</strong> Under Water. Should the<br />

bridge incorporate elements other than those ind icated, these<br />

can subsequently be added to the fonn. Any fau lts or defects<br />

should be commented on so that they can be rect ifi ed by the<br />

next inspection. One should check that the elements have been<br />

recorded as us ing the correct material, have been allocated the<br />

correct type description and, ifneed be, axes.<br />

6. All elements included in an inspecti on shall be checked <strong>for</strong> pos<br />

sible damage which should then be described <strong>for</strong> each element<br />

with the use of damage designations. In each instance the degree<br />

and the consequences of the damage is to be assessed. I freIe<br />

vant, the damage can be illustrated by taking a photograph.<br />

7. Ifpossible, provide the cause(s) of the damage.<br />

8. Proposed maintenance measures and when these will be carried<br />

out must be described <strong>for</strong> all damage of level m 2. Procedure<br />

Nos. 87 and 88 in Norwegian Public Roads Admini stration<br />

Manual No. 026: ' Procedural Code - 2. 1997' \ .... ill be of assitance<br />

in describing these measures.<br />

9. Esti mates should be drawn up <strong>for</strong> each proposed pi ece of main<br />

tenance based on the extent of the damage and the unit cost. The<br />

extent of the damage, i.e. size and quantity, should be noted on<br />

the fonn during the in spection.<br />

10 The results of any measurements and materials testing should<br />

be presented as indicated in Chapter 8.4 'Measurements' and<br />

Chapter 8.5 'Materials Testing'.<br />

II. A Special In spection (see Chapter 6.7) is to be recommended if<br />

Routine <strong>Inspections</strong> uncover a great need <strong>for</strong> repairs or are not<br />

sufficient fo r determining the kind of damage, its consquences,<br />

extent or cause(s). A note should be made of the measure<br />

menls/materials testing to be undertaken, the degree to which<br />

this should be done and the localion(s).<br />

12. The results of the inspection should be recorded in BRUTUS<br />

International at the conclusion of the inspection.<br />

13. Ifrequired the inspection and maintenance plans may be adjusted.<br />

118<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


After carrying out a major inspection of a larger bridge it could be<br />

advisable to produce an expanded report in which the inspection<br />

<strong>for</strong>m represents just one part of the report. It should contain a more<br />

detailed description of any damage, the operational and maintenance<br />

measures and an estimate of the costs. The report can build<br />

on the relevant points suggested <strong>for</strong> drafting reports of Special<br />

<strong>Inspections</strong> - see Chapter 8.3 'Special <strong>Inspections</strong> '.<br />

8.3 Special <strong>Inspections</strong><br />

As much as possible a Special Inspection should act as a good<br />

basis <strong>for</strong> choosing the correct maintenance strategy, describing the<br />

associated measures stating the scope, when they are to be carried<br />

out, and the costs.<br />

Thus it is important fo r the report to be given a struct ure and content<br />

which will <strong>for</strong>m an unequivocal basis fo r prioritising and<br />

assessing the suggested measures. The fo llowing sec tion there<strong>for</strong>e<br />

provides suggestions as to the contents of a Special Report. In<br />

each individual case an assessment should be made of the points to<br />

be included and of how comprehensive each point is to be. When<br />

making use of external inspectors prior agreement SllOU ld be<br />

reached about the extent of the report itself.<br />

1. Summary<br />

2. Introduction<br />

* Summary of the scope of the investigation and t.he damage.<br />

* Specification of the cause(s) of the damage and the mechanisms<br />

leading up to it.<br />

* Required measures, descriptions thereof, time frame, and<br />

fi nancing.<br />

* Recommendations <strong>for</strong> fu rther work<br />

* Name of owner/principal<br />

* <strong>Bridge</strong> number and name<br />

* Name of the consultant<br />

* A description of the purpose of the inspection including refer<br />

ence to the particulars of any damage.<br />

* A description of the extent of the investigation together with<br />

which elements have been included.<br />

3. -Basic Dat a of the<br />

<strong>Bridge</strong><br />

3.1 -Description of the<br />

<strong>Bridge</strong>/ Elements<br />

* Geographical posi tion of the bridge<br />

* Yea r of construction; possibly also the builder and the engineer<br />

ing consultant.<br />

* <strong>Bridge</strong>'s design and principal geometric measurements.<br />

* Special elements<br />

* Materials em ployed<br />

* Design Loads and Service Loads<br />

The BRUTUS International's <strong>Bridge</strong> Card contains most of these<br />

data and can thus be used as an appendix to the report.<br />

<strong>Handbook</strong> <strong>for</strong> Bri dge <strong>Inspections</strong> 119


3.2 - Accessible<br />

Documentation<br />

3.3 location System<br />

4. Descriptio n of<br />

Condition<br />

4.1 Introduction<br />

4.2 Visually Recorded Da ta<br />

4.3 Measurements<br />

4.4 Materials Testing<br />

Accessible documentation can be like:<br />

• Drawings<br />

• Descriptions<br />

• Calculations<br />

• Previous inspection reports<br />

- mention should be made of who undertook the inspection<br />

together with a highlighting of the main findings.<br />

• Documentation from the execution of the inspections like:<br />

- Special conditions surrounding the bridge's construction<br />

- Load conditions during the construction phase<br />

- Relevant infonnation given during construction meet<br />

ings, drawings etc. including speciali st infonnation rele<br />

van! in assessing the development of any damage.<br />

- Pi les records/minutes<br />

- Documentation concerning the surface treatment<br />

- Weather conditions during the construction period<br />

Steel: • Certi ficates <strong>for</strong> the materia ls used .<br />

• Documentation of the checks carried out<br />

on the welding.<br />

Concrete: • Composition<br />

• Conditions during casting process<br />

• Requirements fo r the hardening process<br />

w/c ratio<br />

• Type of cement and quantity used<br />

• Aggregates<br />

• Add itives<br />

• Type of<strong>for</strong>mwork used<br />

• Description oflhe axis numbering system with reference to<br />

appended drawings.<br />

• Time oflhe inspection<br />

• Weather conditions<br />

• Access equipment<br />

• Brief description of the scope and execution of the inspection<br />

• Extent to which consultants were employed<br />

• Data recorded should be allocated to the relevant elements<br />

• Visuall y recorded data should be described with reference to<br />

annexed photographs and sketches<br />

• The level and consequence(s) of any damage should be assessed<br />

in accordance with the codes deta il ed in Chapter 5 -<br />

" Damage Evaluation Fundamentals"<br />

• One summary of the resu lts per type of measurement taken<br />

should be drawn up and included as an annexe. The summary<br />

should be edited after the location has been fix ed.<br />

• One summary of the results per type of materi als test undertaken<br />

should be drawn up and included as an annexe. The summary<br />

should be edi ted after the location has been fixed.<br />

120<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


4.5 Statistical Background<br />

4.6 Submission of Reports<br />

to BRUTUS<br />

5. Damage Assessment and<br />

the Measures Re quired<br />

6. Description of the<br />

Measures to be taken a nd<br />

Main Costs<br />

7. Alternative Repair<br />

Strategies<br />

Appendices<br />

• The scope and results of any specially required calculations<br />

shou ld be described.<br />

• Any ass umptions used in the calculations should be given.<br />

• The results of any stati stical calcul at ions should be presented<br />

with the complete set of calculations included as an annexe.<br />

• This includes a full y completed BRUTUS inspection <strong>for</strong>m.<br />

• The fOnTIS <strong>for</strong> any measurements or materials testing should<br />

also accompany the inspection fOnTI.<br />

• The scope and cause(s) of any damage together with the<br />

measures required to be taken should be assessed on the bas is of<br />

the data collected and the tests undertaken.<br />

• It is recommended that the li me required <strong>for</strong> any necessary<br />

repairs reflects the degree of damage.<br />

• The description should be di vided into secti ons corres ponding<br />

to the elements involved.<br />

• The grouping together of different types of damage requiring<br />

repair measures and their attendant degree and consequence(s)<br />

should be arranged according to the recommended time <strong>for</strong> car<br />

ry ing out the repairs.<br />

• [n accordance with Brutus International' s<br />

'Guidelines <strong>for</strong> the Management, Running and<br />

Maintenance of <strong>Bridge</strong>s' alternative repair strategies must be<br />

presented on the basis of the description of the measu.res to be<br />

taken and their associated costs.<br />

• These strategies should incorporate costs 10 the road user and<br />

other possibl e costs 10 the community should these prove re le<br />

vant.<br />

• An assessment shou ld be drawn up of the existing remaining<br />

lifespan of the bridge, the lifespan after completing tbe repairs<br />

and the costs of demolishing/rebui lding the bridge.<br />

• (Net) present day va lues should be calculated fo r the di ffe rent<br />

strategies, discounted over 25 years using the prevailing rea l<br />

rates of interest.<br />

'" Grouping of the strategies<br />

A Small-sca le (and poss ibly detailed) drawings of the rele<br />

vant elements.<br />

B Measurements - refer to Chapter 8.4 <strong>for</strong> present.ation and<br />

results.<br />

C Material s Testing - refer to Chapter 8.5 <strong>for</strong> presentation<br />

and results.<br />

o Photographs accompanied by comments taken from visua l<br />

records.<br />

E Any necessary statistical analyses.<br />

F Any necessary drawings relating to the descripti_on(s) of<br />

the proposed repa irs.<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 121


8.4 Measurements<br />

Forms have been developed in BRUTUS <strong>for</strong> recording the follow·<br />

ing measurements:<br />

* Levelling<br />

* Horizontal distances/di splacement<br />

A <strong>for</strong>m <strong>for</strong> general use is avai lable <strong>for</strong> other measurements.<br />

The <strong>for</strong>ms are based on Microsoft Excel spreadsheets linked to the<br />

BRUTUS International inspection module. The identity of a bridge<br />

is transferred directly from BRUTUS International when a new<br />

measuremenl fonn is drawn up. An already existing Excel <strong>for</strong>m<br />

containing previous measurements should continue to be used<br />

<strong>for</strong> recording new measurements of the same type.<br />

Recording and Making<br />

Reports<br />

The foll owing data must be recorded and reported:<br />

* Date when measurements were taken<br />

* Which type of ins peel ions the measurements relate to<br />

* The intervals at which the measurements were taken, especially<br />

if this deviates from the inspection intervals<br />

* Those taking the measurements and, possibly, the person ulti<br />

mately responsible <strong>for</strong> them<br />

* Time/temperature/weather conditions. Additionally, <strong>for</strong> levelling<br />

the following factors should be included:<br />

measuring horizontal distances/displacement<br />

height of sag<br />

vertical distances<br />

headroom<br />

* Type of measuring equipment used<br />

* Other comments such as special weather conditions, deviations,<br />

and other infonnation which could be important <strong>for</strong> interpreting<br />

the results<br />

* Location on tbe bridge wbere the measurements were taken - see<br />

Chapter 2.4 " Location of Measurements".<br />

* Results of the measurements<br />

It may be worthwhile presenting the results of, fo r example, a<br />

Special Inspection in an extended report incorporating tables and<br />

visual di splays. After levelling has been carried out, profiles could<br />

be portrayed both lengthways and transversely; the results can be<br />

shown together with previolls measurements and even theoretical<br />

values.<br />

The results of measurements taken should be di scussed and<br />

assessed and will then fonn part of the process of establishing the<br />

degree of any damage, its consequences and cause(s).<br />

122<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


8.5 Materials Testing<br />

As with measurements, BRUTUS International also contai ns<br />

specific Excel based fo rms fo r recording the results of the fo llowing<br />

materials testing:<br />

* Locating rein<strong>for</strong>cement elements/surface cover of concrete<br />

* Measuring the depth of carbonisation<br />

* Measuring chloride content<br />

A general fonn is ava il able <strong>for</strong> recording other types of materials<br />

test ing.<br />

The following data must be recorded and reported on:<br />

Recording and Making<br />

Reports<br />

* Date of the materials tests<br />

* Which type of inspection the materials testing is associated with<br />

* Those conduct ing the materials testing and, possibly, the person<br />

ultimately responsible <strong>for</strong> them<br />

* Temperature and weather conditions<br />

* Method(s) and eq uipment employed, possibly also making ref<br />

erence to Norwegian Pub lic Roads Administration Manuals<br />

Nos. 0 14:'Laboratory Testing ' and 0 15:'On Site Testing'<br />

* Remarks, <strong>for</strong> example concerning the surface treatment, devia<br />

tions and other in fonnation with special significance <strong>for</strong> assess<br />

ing the results<br />

* Location of the materials testing, e.g. which elemeot(s)/axis<br />

reference - see Chapter 2.4 ' Location System'<br />

* The results of materials testing<br />

Figure 8.5- 1 shows examples of the symbols which may be used to<br />

illustrate the different kinds o f tests in drawings and sketches.<br />

Symbols and Type of Testing<br />

® Test site (Bk, Kp, Kd, Oh)<br />

@ Photograph No.3<br />

r,;:;....., Area with a surface cover less than 10 mm<br />

'--'V<br />

Kd3 =5 In Test Area 3 the depth o f carboni sation is 5 mm<br />

Od2 The surface cover <strong>for</strong> Test Area 2<br />

Kp2 The chloride profile <strong>for</strong> Test Area 2<br />

Oh2 Material cut from Test Area 2<br />

Bk6 Core No.6<br />

Figure 8.5-1: Ewmples oflhe symbols which maybe IIsed 10 ilIlls/Y(I/e difJerel1l<br />

killds of tests<br />

<strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong> 123


The test sites of materials test ing co nducted during a Specia l<br />

Inspection should be collective ly illustrated in drawings or sketches<br />

as indicated in Figure 8.5-2.<br />

Numbering the Tests<br />

Presenting the Results<br />

The tests are to be numbe red fo r each element tested, e. g. <strong>for</strong> each<br />

column. So far as columns are co ncerned Test No I sho uld be th e<br />

one conducted lowest down the co lumn with the numbers all ocated<br />

in ascending order moving up each co lumn.<br />

If, fo r examp le, measuring the surface cover, the depth of carbonisatlon<br />

and the chloride content have all bee n conductedsimultaneously,<br />

then the results should be prese nted in a table in such a way<br />

that al l the results from each particular test site can be co mpared.<br />

The assumed cement content should be given in kg/m3 of concrete.<br />

The co nversion facto r <strong>for</strong> the chl oride content of co ncrete by<br />

weight to the chloride content of ce ment by weight shoul d also be<br />

indicated. In the foll owing calculation the specific weight of the<br />

concrete is taken as 23 00 kg/m3<br />

Altiluoa -k. + I 0,0<br />

J<br />

0 4 .1"'1<br />

I<br />

o 2·IOd/KI>'OhJ<br />

®<br />

~ 3<br />

2<br />

.l0.]:; r<br />

1.(0d/Kp)<br />

0<br />

3<br />

,.on<br />

4<br />

,, 117S l<br />

> .<br />

Su~No.4<br />

Surtace No.3 (West)<br />

•<br />

(South)<br />

~II _ '"_No.'<br />

.. (North)<br />

Test<br />

"<br />

Assumed Volume of Cement XlCI kWm'<br />

Conversion Facto< 7.67<br />

Figure 8.5-2: Presenlalion ofTesl Areas & Resulls<br />

124<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


Drilling cores<br />

In this instance an exception can be made concerning the nurn·<br />

bering system already mentioned above. Cores removed by<br />

drilling could, <strong>for</strong> example, be consecutive ly numbered <strong>for</strong> a<br />

whole bridge. The number should be fottowed by a further <strong>for</strong>m<br />

of identification to show where the test was taken:<br />

Bk I (A3+ I 0): Core No. 1 taken from the superstructure al ong<br />

axis No.3 + 10 m.<br />

- 45 %<br />

-E 40 %<br />

35 %<br />

'" 30%<br />

:;; 25 %<br />

'" c:<br />

" =><br />

'"<br />

-0 20%<br />

" 0><br />

'"<br />

15 %<br />

c: 10 %<br />

u<br />

-" 5%<br />

"-<br />

0 %<br />

Bk2(P5):<br />

Core No. 2 taken from Column (Pillar) No<br />

'4 Covering of Assembly<br />

~ Rods as described<br />

,---- I<br />

,---- :.-<br />

Covering of Static Rein<strong>for</strong>cement<br />

I<br />

,<br />

-<br />

as described<br />

.11.<br />

Interval <strong>for</strong> Surface Cover in mm<br />

Figllr€ 8. 5-3: Dis/ribll/ioll of/he SlIrface Cover<br />

Presentation of Chloride<br />

Profiles<br />

""<br />

.l:! )'00<br />

•<br />

,<br />

h "<br />

•<br />

E 1.00<br />

0<br />

~ 1-'0<br />

u<br />

~ 1.00<br />

."<br />

"00 ,<br />

'"<br />

""<br />

], 1-'0<br />

~<br />

, W><br />

•<br />

8 1-'0<br />

" v 1.00<br />

• ""<br />


It is important thaI the resul ts of materials testing are presented in<br />

such a way that they are eas ily understood. The fo llowing shows<br />

examp les of how the results of ordinal)' materials testing of concrete<br />

were presented.<br />

Figure 8.5-3 shows the distribution of the surface cover of the rein<strong>for</strong>cement<br />

in the superstructure, Area I ofGimseystraumen <strong>Bridge</strong><br />

in Norway. The distribution results are based on 2029 indi\' idual<br />

measurements.<br />

Figure 8.5 A illustrates examples of the presentation of chl oride<br />

profiles <strong>for</strong> Ihe central section of Area 1,5 metres from Axis No .2<br />

in the superstructure ofGimsoystraumen <strong>Bridge</strong> in Norway.<br />

potential readings (mV CS E)<br />

25 125 225 32S 425 525 625 725 825 925<br />

0, 12 - 135 -131 -140 -74 -21 -8 -32 -120 -101<br />

100: -83 -84 -84 -85 -71 -30 7 -68 -31 -III<br />

200 : -9' -114 -83 -58 -51 -2] -IS -34 -10 I -79<br />

300 : -75 - 158 -99 -68 -101 -100 -35 -68 -105 -87<br />

400: -4' -110 -75 -60 -42 -100 -32 -38 -92 -102<br />

500 : -130 -215 -163 -117 -119 -56 -23 -64 -75 -42<br />

600, -9 1 -209 -57 -97 -112 -112 -65 -71 -96 -77<br />

700 : -90 -170 -74 - 11 4 -71 -67 -60 -40 -67 -147<br />

800 : -134 - 182 -156 -114 -80 -33 -45 -44 -72 -47<br />

900 : -40 - 122 -121 -82 -43 -40 -45 -89 -88 -55<br />

a) Minorcritical colorcombination<br />

potent ial readings (mV CSE)<br />

25 125 225 32S 425 525 625 725 825 925<br />

0, 12 - 135 -1]1 -140 -74 -21 -, -32 - 120 -101<br />

100: -83 -84 -84 -85 -71 -30<br />

,<br />

-68 -31 -III<br />

200 : -9' -114 -83 -58 -51 -23<br />

-34 -10 I -79<br />

300 : -75 -158 -99 -68 -101 -100 -35 -68 -105 -87<br />

400: -4' -110 -75 -60 -42 -100 -32 -38 -92 -102<br />

500 : -I ]0 -215 -16] -117 -119 -56 -23 -64 -75 -42<br />

600, -91 -209 -57 -97 -112 -112 -65 -71 -96 -77<br />

700 : -90 - 170 -74 -1 14 -71 -67 -60 -40 -67 - 147<br />

800 : -I ]4 - 182 -156 - 11 4 -80 -33 -45 -44 -72 -47<br />

9o,,, -40 - 122 -121 -82 -43 -40 -45 -89 -88 -55<br />

b) Most possible colorcombination<br />

potent ial readings (mV CS E)<br />

25 125 225 325 425 525 625 725 825 925<br />

0, 1 ' -135 -131 -140 -74 ' 1 -, J:I -120 -101<br />

100: -83 -84 -84 -85 -71 ~() 7 -68 -31 -III<br />

200 : -9' -114 -83 -510: -51 -2J -IS<br />

-101 -79<br />

]00 : -75 -158 -99 -6, -101 -100 J5 -68 -105 -87<br />

400: -44 -110 -75 -60 -42 -100 12 -lK -92 -102<br />

500 : -I ]0 -215 -16] -117 -119<br />

-2] -64 -75 -42<br />

600 : -91 -209 ·57 -97 -112 -112 " -65 -71 -96 77<br />

700 : -9' -170 -74 -114 -71 -67 -60 40 -67 -147<br />

800 : -134 -182 -156 -114 -80 -33 -45 -44 -72 -4'<br />

90


ECP-Measurements<br />

For the presentation of potential readings (ECP) the<br />

drawings/sketches should clearly indicate where the measurement<br />

was taken <strong>for</strong> each element and the location of the earthing point.<br />

EC P readings should be interpreted in accordance with Report<br />

No.94-l 6 issued by the Norwegian Publ ic Roads Administration,<br />

<strong>Bridge</strong> Di vision: ' Recommendations <strong>for</strong> the Use of<br />

Electrochemical Equipment <strong>for</strong> Measuring Potential'. The in terpretati<br />

on should include, amongst other things, the requirement<br />

<strong>for</strong> three different versions according to co lour setti ng;<br />

Less cri tical colour setting than (b)<br />

Colour choice considered to be the best<br />

More critical colour setting than (b)<br />

Exampl es of the above are shown in Figure 8.5-5.<br />

8.6 Presentation of Damage<br />

Drawings and Sketches<br />

For the reporting of visual inspections drawings/sketches can be<br />

made showing the location and scope of the different kinds of<br />

damage which are in ev idence. This can prove to be an extensive,<br />

time consuming task and should only be undertaken in very special<br />

circumstances.<br />

One exception will be the presence of serious, special sc ratches<br />

and fissures which have to be photographed and/or drawn in on<br />

sketches stating thei r total, the distance from each other and their<br />

length. Both the maximum and average opening of these scratches<br />

and fissures should be indicated.<br />

The symbols which can be empl oyed in draw in gs <strong>for</strong> each Iype of<br />

damage are presented in Figure 8.6- 1.<br />

w •<br />

Casting j Oint<br />

Delam ination, spalling<br />

Po ro usa r bad qu a Ii ty co n crete<br />

_.<br />

0,2 m m ,2,O mm<br />

Cracking<br />

V isi b Iy co rrod ing rein fa ree ·<br />

ment<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 127


128 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9 DAMAGE EVALU­<br />

ATION CATALOGUE<br />

The detailed list of the different categories of damage is intended<br />

to assist in the assessment of the significance of any damage to<br />

individual bridges in ajustifiable and proper manner.<br />

Sub-chapters<br />

The list has been divided into Ihe fotlowing II sub-chapters which<br />

deal with types of damage to different materials and to the usual<br />

elements and accessories fou nd on a bridge.<br />

9. 1 Elements in or on Ihe Ground<br />

9.2 Concrete Elements<br />

9.3 Steel Elements<br />

9.4 Masonry Elements<br />

9.5 Timber Elements<br />

9.6 Wearing surfaces/insu lat ion against dampness<br />

9.7 Bearings with bearing shelflbearing shelf<br />

9.8 Joints/joint threshold<br />

9.9 Raili ngs & parapets<br />

9.10 Dra inage system<br />

9. 11 Other items of equipment<br />

Each of the above elements are in turn subdivided into the different<br />

types of damage - refer to Chapter 5.2 "Types of Damage".<br />

The following standard layout should be used <strong>for</strong> each type of<br />

damage:<br />

Description<br />

Ca use of Damage<br />

Re leva nt<br />

Measu rements/Materials<br />

Testing<br />

Degree of Damage and the<br />

Consequenses<br />

Condition w hich trigger<br />

Maintenance Works<br />

Action to be ta ken<br />

Examples<br />

Explanation of the damage in question<br />

Possible causes of the damage ari sing<br />

Measurements /materials testing which ought to be undertaken in<br />

order to discover hidden damage, to ascertain its scope and to project<br />

future developments and/or propose possible causes of damage.<br />

Description of how to evaluate the seriousness and consequences<br />

of the particular type of damage.<br />

Requirements and recommendations concerning the condition<br />

which can trigger maintenance work . A degree of damage':::"2 is<br />

requ ired as a minimum.<br />

Suggested action needed to fo llow up a damage or repa ir it.<br />

Most of the types of damage will be described with illustrat ions.


9.1 Elements in or<br />

on the Ground<br />

These elements are detailed in Chapler 2.2 'Types of Elelnents',<br />

and the following types of damage can be found.<br />

Damage<br />

101 Subsidence of ground/embarkments<br />

102 Obstruct ion of waterway<br />

103 ScouringlErosion of river course<br />

104 Inadequate cleaning up/removal procedures<br />

109 Other Iypes of damage/defects<br />

Page<br />

13 1<br />

133<br />

135<br />

14 1<br />

143<br />

The above items will now be described more fully.


9.1 ELEMENTS IN THE GROUND<br />

101. Subsidence of Ground/Embarkments<br />

Description<br />

Vertical movements in the soil behind abutment, wing walls and infill etc. which do not affect the<br />

bridge itself.<br />

Degree of Damage<br />

Error during the planning phase. The load capaci ty oflhe soi l has been overestimated .<br />

• Incorrect material(s). Wrong compos ition of material has been used in the backfill.<br />

'" Work incorrect ly exec uted - not as origina lly described.<br />

* Loads. Traffic causes overloading.<br />

'*' Damage caused by accidents, e.g. flooding<br />

'" In-service damage, e.g. the results of erosion.<br />

'" Relevant Measurement<br />

* Levelling<br />

'" Evenness<br />

Degree of Damage/Consequences of the Damage<br />

The degree of damage should be selected based on its scope and probable rale of development.<br />

Basically subsidence can be of significance fo r traffic safety, maintenance costs and the environment.<br />

In fact subsidence behind abutment piers can result in differences in the height of the road<br />

surface where intill and pavement meet. This in turn has implications <strong>for</strong> traffic safety. Height diffe<br />

rences can also lead to impact in the joints and consequent noise pollution <strong>for</strong> those living in the<br />

vicin ity of the bridge.<br />

Conditions Triggering Maintenance Measures<br />

The inspector must assess each case indi vidua lly. If the lengthwise height difference <strong>for</strong> the carriageway<br />

on a main road exceeds 20 mm (or 30 mm <strong>for</strong> other national roads) when measured with a<br />

2m long straightedge, then the necessary maintenance measures should be set in motion.<br />

Maintenance Measures<br />

* Fill in with sui table material(s)<br />

* Small differences in he igh t can be evened out with asphalt<br />

• If the subsidence continues then consideration should be given to replacing the entire inti II<br />

behind the abutment.


9.1 ELEMENTS IN THE GROUND<br />

Example9.1-1<br />

Subsidence or the infill behind the abutment pi er<br />

has caused a difference in height of27 mm in the<br />

road surface. The bridge is situated on a main road<br />

and subject to a lot ofhcavy traffi c. The gap has<br />

resulted in noise pollution <strong>for</strong> those li ving in the<br />

vicinity of the bridge. The damage has affected<br />

both traffic safety and the environment.<br />

Type of Damage:<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

101 Subsidence<br />

3T,3M<br />

61 Traffic Loads<br />

Procedures:<br />

Fill with asphalt within I year.<br />

Example 9.1-2<br />

Severe subsidence of the bark infi ll with a resultant<br />

large difference in height between the bridge and<br />

the inti I\, The damage is to be considered as dangerous<br />

<strong>for</strong> traffic, and the subsidence has also affected<br />

Ihe appearance of the wall underneath the bridge.<br />

The di splacement of the columns indicates that the<br />

pressure exerted by the earth has cause additional,<br />

great strai n on them.<br />

Type of Damage:<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

of Materials<br />

101 Subsidence<br />

3T,2M<br />

II Incorrect Choi ce<br />

Procedures: Replacement of the material with, <strong>for</strong><br />

example, EPS. The condition of the columns must<br />

be carefully checked after removal of the old material.<br />

Example 9.1-3<br />

Subsidence o f the earth under a small part of a<br />

wing-wall. This can affect load bearing capacity<br />

should the subsidence develop.<br />

Type of Damage:<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

101 Subsidence<br />

2C<br />

9 Other/Unknown<br />

Procedures:<br />

5 years.<br />

Fill with appropri ate material within


102. Obstruction of Waterway<br />

9.1 ELEMENTS IN THE GROUND<br />

Description<br />

The accumu lation of debris, branches, driftwood and the like have resu lted in constrictions in drainage<br />

cul verts. The speed of the water flow will consequently increase, and the slate of the current<br />

will also change; this can in turn lead to erosion and scouring.<br />

Cause of Damage<br />

'" Insufficient regular management/maintenance; insufficient clearing out of the drainage culvert.<br />

'" Accidental damage, e.g. flooding.<br />

Degree of Damage/Consequences of the Damage<br />

Since erosion and scouring can very qui ckly result from constrictions in drainage culverts, the<br />

degree of damage should normally be given a high score.<br />

Constricti ons can affect the bridge's load bearing capacity, traffic safety and maintenance costs as<br />

fo llows:<br />

'" Increased risk of erosion and scouring leading to reduced load bearing capacity and consequently<br />

to increased maintenance costs.<br />

* A combination of damming up and breaking up of ice particularly can lead to the water flooding<br />

over the road, thus affecting traffic safety.<br />

Conditions Triggering Maintenance Measures<br />

Routines should be established <strong>for</strong> clearing river courses. In the event of constrictions arising the<br />

need <strong>for</strong> remedial measures should be assessed in each case. This wi ll depend on, amongst other<br />

th ings, the degree of the constriction and whether the drainage culvert has extra capacity or not. The<br />

necessary measures should be taken be<strong>for</strong>e directly related damage arises.<br />

Maintenance Measures<br />

• Clear out the drainage culvert<br />

* Restore the ori ginal water course<br />

* Special action required <strong>for</strong> damming up


9.1 ELEMENTS IN THE GROUND<br />

Exa mple9.1-4<br />

The complete water course has been fi lled with<br />

debris from bushes and trees. The bridge is situated<br />

above a typical flood course. It has, however, satisfactory<br />

enough foundations such that there should<br />

be no danger of scouring. The constrictions can<br />

have consequences fo r the maintenance costs if the<br />

water runs out over the road into the material<br />

behind the abUlmenl pier which is then displaced.<br />

Type of damage:<br />

102 Obstruction of<br />

waterway<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

nmg.<br />

Procedures:<br />

Thorough cleaning out within 1 year.<br />

3M<br />

44 Insuffi cient clea-<br />

Example 9. 1-5<br />

Rubbish bui ld-up in the drainage culvert. There is a<br />

risk orlhe material around the pipe sufferi ng from<br />

scouring after a flood. The load bearing capacity of<br />

the bridge and the maintenance costs can conse~<br />

quent ly be affected.<br />

Type of Damage:<br />

waterway<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

nmg.<br />

102 Obstruction of<br />

2C.3M<br />

44 Insufficient clea~<br />

Proced ures:<br />

Thorough cleaning out within I year.


9.1 ELEMENTS IN THE GROUND<br />

103. Scouring/Erosion of River Course<br />

J~~~~ ~~:'" '" ABOVE WATER<br />

,- 1... ______ _<br />

OR IGINAL LEVEL<br />

........ 1<br />

1... ________ -'<br />

CAUSED BY SURFACE<br />

WATER<br />

Description<br />

Damage in th is category includes erosion oflhe earth both above and below the water line. An<br />

exampl e of the latter could be erosion of the natural river bed or of protection against erosion. If the<br />

erosion is not stopped in time the fou ndations will become under-scoured. On the other hand damage<br />

above the water line can be exemplified by erosion of embankments and slopes in the immediate<br />

area of abutments and columns.<br />

Cause of Damage<br />

Some of the possible causes are as fo llows:<br />

• Faulty design: During the plann ing period inadequate development or lack of attention paid to<br />

the draining ofT of surface wate r. inadequate design of a bridge can result in a narrowing of<br />

the waterway and a consequent increase in water speed.<br />

• Faulty construction: not carried out as prescribed<br />

• Unsatisfactory day-to-day run ning/maintenance; Damming up of the water course due to the<br />

accumulat ion of branches and other debris.<br />

• Accident impact; Erosion/scouring caused by severe water discharge from fl ooding.<br />

• In-service damage; For example the results of changes to the water course fo ll owing work carri<br />

ed out on the ground in the vicinity.<br />

Degree of Damage & its Consequences<br />

Erosion below water level should be all ocated a high degree of damage because it can develop very<br />

quickly. Even small movements of earth around foundati ons can affect the carrying capacity.<br />

Erosion can qui ckly turn into scouring. The degree of damage fo r situations above the water level<br />

should be assessed based on the local conditions and probable developments.<br />

Un derwater erosion can affect both carry ing capacity and maintenance cost.<br />

Carrying Capacity<br />

• Erosion around a bridge opening can reduce the carrying capacity of the foundations when the<br />

earth around them is removed. Foundations without pi les are especiall y vul nerable, and the risk<br />

of under-scouring is great - please refer to th e drawing above. Base slab foundations will always<br />

lose carrying capacity when subjected to underscouring with resultant subsidence.Subsidence in<br />

the foundations produces de<strong>for</strong>mation of the superstructure and can lead to the partial or ful l col<br />

lapse of the bridge in question.


9.1 ELEMENTS IN THE GROUND<br />

•<br />

Clfklinallevel<br />

V<br />

, \ •<br />

-<br />

V<br />

V<br />

V •<br />

/<br />

B<br />

~<br />

- ~ -<br />

""'"'"<br />

/' • V<br />

• V •<br />

7<br />

vi<br />

1,5 m<br />

Foundations on piles do not no rmally need ea rth masses under the foundations to achieve carrying<br />

capacity. Free-standing piles, on the other hand, will be vu lnerable to damage from ice, dtifnvood,<br />

rot and should there<strong>for</strong>e be protected. The figure above is based on the <strong>for</strong>mulae <strong>for</strong> calculating carry<br />

ing capacity detailed in the <strong>Bridge</strong> Manual and demonstrates how carrying capacity is reduced<br />

from 100% (at the original levei 'A ') to 50% (at new level 'S') when erosion. Should the erosion be<br />

allowed to continue up to level 'C', th en carrying capacity will be reduced to 25% of the o:riginal<br />

figure.<br />

Maintenance Costs<br />

Even minor damage to protective measures against erosion show a tendency to accelerate and become<br />

expensive to repair. It is important that protection against erosion be in working order especially<br />

in a flood situation, otherwise scouring can arise with resultant severe co nsequences <strong>for</strong> the carrying<br />

capacity. Erosion above water level can offect the carrying capacity, traffic safety, majntenance<br />

and the environm ent. The removal of earth masses from around abutment piers can lead t() reduced<br />

carrying capacity. Erosion can produce holes in the pavement wi th resultant risk to road users. The<br />

scope of the damage can increase markedly if measures are not taken to halt the erosion.<br />

L-<br />

Conditions which Trigger Maintenance Measures<br />

Maintenance measures must be undertaken immediately when erosion and particularly under-scouri<br />

ng of foundations have occurred underwater. Cases of erosion above the water line should be individually<br />

assessed by the inspector.<br />

Maintenance Measures<br />

Undenrarer :<br />

• Flushing out the water course<br />

• Repair of damaged erosion protection<br />

• Construct erosion protection<br />

• Replenishing earth masses below and around foundations with suitable material<br />

• Recasti ng of concrete under the foundations if the carrying capacity enables so. Found alions<br />

supported on pi les should be given special attention.<br />

Above /Va/erLeI'e1<br />

• Replenishing with suitable new materia ls<br />

• Covering em bankments w ith paving stones<br />

• Improvements to the drainage system directed fonvards removal of surface water.<br />

• Sowing seeds/planting to encourage binding of the soil.


9.1 ELEMENTS IN THE GROUND<br />

Original Level<br />

~-..I....- \--1" .f-:7--.~<br />

/ :""<br />

. r . 9~· ~ ~<br />

\le'/el after Erosion<br />

Example 9. 1-6<br />

The original undenvater ground level has been eroded<br />

down to the same level as the bottom of the<br />

base foundation slab due to insufficient protection<br />

against erosion.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

3C<br />

Cause of Damage: 13<br />

Poor design solutions<br />

Procedures: Replenish with suitabl e materials and<br />

install protection against erosion within one year.<br />

•<br />

,<br />

Original level<br />

\ " •<br />

•<br />

"<br />

•<br />

• "<br />

"<br />

•<br />

Level after Erosion<br />

~<br />

Example 9. 1-7<br />

The original underwater ground level has altered<br />

due to erosion with severe consequences <strong>for</strong> the<br />

carrying capacity. The ba ll ast co nsists of too fine a<br />

grade of material.<br />

Type of Damage:<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

Construction fa ult<br />

103<br />

4C<br />

38<br />

Procedures: Replen ish wit h suitab le materials and<br />

install protection against erosion in the course of<br />

s ix months.<br />

Example 9.1-8<br />

The base foundation slab has suffered under-scouring<br />

as the result of a serious flood. Carrying capaci<br />

ty has been greatly reduced.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

4C<br />

Cause of Damage: 73<br />

Flooding<br />

Procedures: The bridge should be closed until<br />

repairs have been carried out" immediate infilling<br />

with concrete under the foundations, replenish ing<br />

w ith suitable materials a nd installing protection<br />

against erosion to the same level as the origi nal<br />

river bed.


9.1 ELEMENTS IN THE GROUND<br />

Example 9.1-9<br />

Under-scouring of foundations on vertical piles<br />

because of insufficient protection agai nst erosion.<br />

Vertical, but not horizontal loads can be accommodated,<br />

whilst the piles can be subjected to un<strong>for</strong>eseen<br />

sources of impact. The consequences <strong>for</strong> the bridge's<br />

carrying capacity arc serious.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

4C<br />

Cause of Damage: 12<br />

Erroneus calculat ions<br />

Procedures: Infi lling with concrete under the foundati<br />

ons, replenishing with su itable matcrials and<br />

installing protection against erosion. This shou ld be<br />

carried out within 6 months.<br />

Example 9.1-10<br />

Erosion of the embankment caused by the water<br />

from the pavement not being drained off as planned.<br />

If the situation is allowed to continue at the present<br />

rate of development, maintenance costs will be<br />

affected. Since a lot of public transport passes under<br />

the bridge, the damage is also of consequence fo r its<br />

appearance.<br />

Type of Damage:<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

Cause of Damage:<br />

Construction fau lt<br />

103<br />

3M,3E<br />

38<br />

Procedures: Infill ing with suitable materials,<br />

improvements to the drainage system and installati ­<br />

on of protecti on against erosion. To be carried oul<br />

during the year in question.<br />

Example 9.1-11<br />

A combination of erosion of the in fi ll behind the<br />

wing-walls and inadequate anchoring of the elements<br />

has resulted in the displacement of the fac ing<br />

slabs at the top edge of the bridge. Consequently<br />

there is a risk of them falling onto the pathway<br />

below the bri dge.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

4T<br />

Cause of Damage: 38<br />

Faulty Construction<br />

Procedures: The elements should be righted and<br />

made safe within 6 months.


9.1 ELEMENTS IN THE GROUND<br />

Example 9.1-12<br />

As a result of erosion some of the concrete blocks<br />

on the front of an abutment pier have started to sl ip.<br />

Settlement and holes have appeared in the infill<br />

behind the abutment pier which in turn has an effect<br />

on traffic safety.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Conseq uences:<br />

4T<br />

Cause of Damage: 38<br />

Faul ty Construction<br />

Procedures: Temporarily repair by immediately<br />

infilling with material and later permanently by<br />

installing a relief plate against the back wall.<br />

Example 9.1-13<br />

A small amount of erosion under an abutment pier<br />

due to lack of attention being paid during the planning<br />

phase to the draining away ofwaler.<br />

Type of Damage: 103<br />

Scouring/erosion of rive r course<br />

Degree of Damage &<br />

Consequences:<br />

1M<br />

Cause of Damage: 13<br />

Poor design solutions<br />

Procedures: None<br />

Example 9.1-14<br />

Erosion has started under an abutmenl pier because<br />

insufficient attention has been paid during the construction<br />

phase to draining water from the roadway.<br />

Ma intenance costs may be affected if the erosion is<br />

allowed to develop.<br />

Type of Damage: 103<br />

Scouring/erosion of river course<br />

Degree of Damage &<br />

Consequences:<br />

2M<br />

Cause of Damage: 38<br />

Faulty Construction<br />

Procedures: Replacement of ballast materials,<br />

improvements to the drainage system and protection<br />

against surface erosion. To be carried oul within<br />

5 years.


9.1 ELEMENTS IN THE GROUND<br />

Example 9.1 -15:<br />

Erosion on the front of an abutment pi er has caused<br />

some of the concrete blocks to start sl ipp ing out of<br />

place.<br />

\<br />

Type of Damage: 103<br />

Scouring/erosion of ri ver course<br />

Degree of Damage &<br />

Conseq uences: 2.\1<br />

Cause of Damage: 38<br />

Faulty Construction<br />

Procedu res:<br />

Improvements to the drainage system, infi ll ing<br />

underneath the flagstones and relaying the flagsta·<br />

nes. To be carried oul within 5 years.


9.1 ELEMENTS IN THE GROUND<br />

104. Inadequate Clearing Up & Removal<br />

Procedures<br />

Description<br />

Included under this heading are the following:<br />

• Insufficient clearing up once construction work is complete<br />

• Failure to remove vegetation under and against a bridge<br />

• Failure to remove materials/equipment stored under a bridge<br />

Cause of Damage<br />

• Construction fauit - insufficient clearing lip once constructi on work is complete<br />

'" Inadequate day-to-day management/maintenance<br />

Degree of Damage/Consequences<br />

The degree allocated to the damage will depend on its type, scope, and the speed at which other<br />

kinds of damage can develop. A hi gh degree of damage should be used <strong>for</strong> new bridges.<br />

Inadequate clearing up and removal procedures can cause further damage which could affect maintenance<br />

costs or the environment. Costs to remove or clear up items are often less than to repair<br />

secondary damage.<br />

Conditions which Trigger Maintenance<br />

Clearing up and removal procedures should be fo llowed immediately after the construction ora<br />

new bridge is complete. For already existing bridges procedures should be effected if inadequate<br />

clearing up or removal of items resulting in damage which could affect ma intenance costs or the<br />

environment.<br />

Procedures<br />

* Clearing up or removal of the items in question


9.1 ELEMENTS IN THE GROUND<br />

Examplc9.1-1 6<br />

Dense vegetation on an abutment pier.<br />

Type of Damage: 104<br />

Inadequate Clearing Up/Removal<br />

Degree of Damage &<br />

Consequences: 3,\1<br />

Cause of Damage: 44<br />

Inadequate Maintenance<br />

Procedures:<br />

The vegetation shou ld be removed within a yea r.<br />

Example 9.t-1 7<br />

Culvert used to store bails of straw.<br />

Type of Damage: 104<br />

Inadequate Clearing Up !Removal<br />

Degree of Damage &<br />

Consequences:<br />

3M<br />

Cause of Damage: 44<br />

Inadequate Maintenance<br />

Procedures:<br />

Clear olil ihe culvert with in onc year.


9.1 ELEMENTS IN THE GROUND<br />

109. Other Types of Damage to River<br />

Course<br />

Description<br />

Th is category includes damage/shortcom ings not already covered in Chapler 9.1 , fo r example the<br />

loads exerted on foundations will increase if infi ll is deposited around them. Excavation work near<br />

to foundations can reduce carrying capacity, whilst the fiver can suffer from erosion in a different<br />

way after excavation of the water course. The foundations can then be put at risk.<br />

This category also includes faults/shortcomings in the soil itself which can also lead 10 damage, <strong>for</strong><br />

example the absence ofwaler training wal ls, or a waterway with insufficient capacity. Additional<br />

examples may have originated from the co nstruction period, such as embankments wh ich remain<br />

unsown or yet to be installed protection against erosion.<br />

Cause of Damage<br />

'" Design fault<br />

'" Construction fault<br />

'" Inadequate daY-Io-day maintenance<br />

Degree of Damage/Consequences<br />

The degree must be assessed against the background of the prevailing local conditions and how<br />

much the damage could develop.<br />

The inspector must assess the consequences.<br />

Conditions which Trigger Maintenance<br />

Action should be taken whenever fau lts/shortcomings can lead to the development of damage<br />

which cou ld affect carrying capacity.<br />

Procedures<br />

These should be assessed in each individual case.


9.2<br />

ConcreteE lem ents<br />

The undernoted types of damage may arise in elements made of<br />

concrete:<br />

No.<br />

Page<br />

201 Settl ement of concrete element 146<br />

202 Movement of concrete element 148<br />

203 De<strong>for</strong>mat ion of concrete element 150<br />

204 Cracks in concrete element 153<br />

205 Rupture of concrete element 160<br />

206 Damage to concrete surface treatment 162<br />

207 Lea kage/dampness of concrete 164<br />

208 Discolorati on of concrete element 168<br />

209 Insufficicnt/damaged cover of concrete element 170<br />

2 10 Weathering of concrete element 173<br />

2 11 Honeycombing of concrete element 176<br />

21 2 Delamination of concrete element 179<br />

2 13 Spalli ng of concrete element 180<br />

2 14 Corrosion of rein<strong>for</strong>cement 184<br />

2 15 Wa sh out of concrete element 188<br />

21 6 Inadequate cl eani ng of concrete element 19 1<br />

2 17 Inadequate Clearing Up/Removal 193<br />

290 Other damage to concrete element 195<br />

Examp les or the above will now follow.<br />

Damage to concrete wearing surfaces is described in Chapter<br />

9.6.2, whilst damage to concrete parapets is dealt with in Chapter<br />

9.9. 1.<br />

<strong>Handbook</strong> <strong>for</strong> Brid ge <strong>Inspections</strong> 145


9.2 CONCRETE ELEMENTS<br />

201 Settlement of Concrete Element<br />

Description<br />

Vertical movements in concrete abutment , wing walls, pillars etc. Sett lement in these eleme nts can<br />

late r lead to defonnation of the superstructure - refer to Type of Damage No. 203.<br />

Cause of Damage<br />

• Design fault - overestimati on of the ground's carrying capacity, underestimati on of the pressure<br />

exerted by the ground<br />

• Material fau lts - incorrect composition of infill material<br />

• Construction faults - fo undations not constructed as agreed<br />

'" Loads - caused by traffic or extra pressure on the ground in connection with construction work in<br />

the vicinity<br />

• In-service damage - secondary damage from erosion or underscouring of the ground.<br />

Current Measurements<br />

• Levell ing<br />

Degree of Damage/Consequences<br />

The degree of damage must be assessed based on the scope of the settl ement and its development as<br />

well as on any damage the settl ement may cause to the element which is subsiding. Both carrying<br />

capacity and/or maintena nce costs can be affected.<br />

146 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9.2 CONCRETE ELEMENTS<br />

Conditions which trigger Maintenance<br />

Action must be taken immediate ly whenever settlement has lead to too Iowa carrying capac ity. For<br />

settl ement which can result in 100 Iowa carrying capacity action must be taken be<strong>for</strong>e this happens.<br />

Action should also be taken in cases where settlement can be of importance <strong>for</strong> maintenance costs<br />

Procedures<br />

. Replacement of infil l wit h a lighter material in order to reduce vertical loads and the pressure<br />

exerted by the ground .<br />

. Constructi ng new foundations usi ng, <strong>for</strong> example, pi les.<br />

Example 9.2-1<br />

Severe settlement of an abutment which is built on<br />

infill. The infi ll material's sensitivity to subsidence has<br />

been underestimated. The abutment has nol been subjected<br />

to any damage whi ch requires repair in the short<br />

term. The superstructure is of the continuous type, and<br />

it has become necessary to temporarily build up the<br />

bearings in order to reduce de<strong>for</strong>mation.<br />

Type of Damage:<br />

Dcgrce of DamagcJ<br />

Consequence:<br />

Cause of Damage:<br />

Procedures:<br />

20 I Settlement (abutment)<br />

203 De<strong>for</strong>mation of concrete<br />

element (Superstructure)<br />

I C <strong>for</strong> the abutment<br />

4C <strong>for</strong> the superstructure<br />

be<strong>for</strong>e the temporary<br />

support<br />

13 Poor design so lutions<br />

No action is required <strong>for</strong> the abutment , but the settlement<br />

should be fo llowed up by us ing levell ing<br />

The de<strong>for</strong>mation of the superstructure was so severe<br />

that the bridge had to be closed to heavy traffic until it<br />

had been jac ked up and the bearings had been bui lt up.<br />

<strong>Handbook</strong> fo r <strong>Bridge</strong> <strong>Inspections</strong> 147


9.2 CONCRETE ELEMENTS<br />

202 Movement of Concrete Element<br />

Description<br />

The movement of bridge elements away from their original position, e.g. horizontal disp lacement<br />

or rotation of abutment , piers or parts of the superstructure. Evidence of movement can o ften be<br />

seen in bearings and joint gaps.<br />

Cause of Damage<br />

... Design fau lts - overestimation of the ground's carrying capacity; earth pressure underestimated .<br />

... Materia l defects - incorrect materials <strong>for</strong> the infill.<br />

... Construction fau lts - foundations not constructed as designed .<br />

... Loads impact from traffic.<br />

• Inadequate day-ta-day operation/maintenance - absence of cleaning measures <strong>for</strong> joints .<br />

... Accident impact, e.g. flooding or traffic impacts.<br />

Current Measurements<br />

'" Measuring th e movements.<br />

Degree of Damage/Consequences<br />

The degree of damage should be fixed based on the size and probable development of the movement.<br />

Please note that movement is more cri tical <strong>for</strong> inclined than straight bridges because of the<br />

sideways di splacement of the superstructure.<br />

Extreme movements can affect the carrying capacity, but nonnally it is the maintenance costs<br />

which are influenced. Protruding edges along the kerb may affect traffic safety.<br />

Conditions which trigger Maintenance<br />

These should be assessed <strong>for</strong> each particular case and wi ll often depend on the relationship between<br />

the move ments whi ch have come to light and the capacity of the bearings and possibl y of the joint<br />

constructions. Furthermore the situation may depend on whether protruding edges represent a<br />

danger to trafiic.<br />

Actions<br />

• Cleaning joints<br />

• Jacking up and adjusting bearings and possibly also building them up<br />

• Replacement of infillmaterial with lighter ones in order to reduce the pressure onthe ground.<br />

148 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9.2 CONCRETE ELEMENTS<br />

Example 9.2-2<br />

Unstable conditions have lead to movement in the<br />

abutment. The joint openings have become completely<br />

closed, and the spalling evident on the abutment<br />

and cross-girders indicates thai the superstructure<br />

is under continuous stress.<br />

Type of Damage: 202 Movement of concrete<br />

element<br />

Degree of Damage &<br />

Conseq uences: 2C<br />

Cause of Damage: 12 Erroreous calculation<br />

Procedures:<br />

Continuous taking of measurement s to fo llow developments.<br />

If these continue the infill behind the<br />

abutment will have to be rep laced within five years.<br />

Example 9.2-3<br />

The backfil l contains frost susceptible materials<br />

below ground level with the resu lt that the abutment<br />

has been subject to movement, whilst the<br />

superstructure has suffered sideways movement<br />

because the connection between the bridge and the<br />

abutment is skewed. There are protruding kerb<br />

edges on the superstructure on the roadway. The<br />

structures' abi lity to withstand the movements is<br />

temporarily suffi cient, and the bridge's carrying<br />

capacity has not yet been affected.<br />

Type of Damage: 202 Movement of concrete<br />

element<br />

Degree of Damage &<br />

Conseq uences: 2M <strong>for</strong> Abutment<br />

3T Superstructure<br />

Cause of Damage: I I Incorrect choi ce of materials<br />

Procedures:<br />

The intill behind the abutment should be replaced,<br />

and the superstructure jacked up within three years.<br />

Example 9.2-4<br />

The pier cap has been deflected 55 mm in a longitudinal<br />

direction during a period of 40 years apparen<br />

tly because of ice loads.<br />

Type of Damage: 202 Movement<br />

Degree of Damage &<br />

Consequences: I C (<strong>for</strong> Piers)<br />

Cause of Damage: 65 Ice impact<br />

Procedures:<br />

Continuous fo llowing up.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 149


9.2 CONCRETE ELEMENTS<br />

203 De<strong>for</strong>mation of Concrete<br />

Element<br />

The type of damage "De<strong>for</strong>mationy" covers bridge elements which have developed bowing whencompared<br />

to their original shape. They can consequently have been subj ected to additional loads or<br />

now have reduced carrying capacity. The consequence can be pennanent deflection of, <strong>for</strong> example,<br />

the main carrying element or the bridge deck etc.<br />

Cause of Damage<br />

• Design fault - under-designed elements or incorrect assumptions.<br />

• Construct ion fault - settlement of the scaffolding during construct ion; unintentionally applied<br />

loads.<br />

• Loads - overloading due to heavy vehicular loads; too thick an asphalt layer.<br />

• Accident impact - traffic colli sions.<br />

• In-service impacts - c.g. secondal)' damage due to subsidence <strong>for</strong> example.<br />

Possible Measurements<br />

• Levelling.<br />

Degree of Damage & Consequences<br />

De<strong>for</strong>mation of load bearing elements can be an indication of too Iowa carrying capacity or of<br />

overloading.<br />

The degree of damage assigned must be based on the severity of the defonnation and its probable<br />

further development.<br />

So far as continuous span bridges are concerned de<strong>for</strong>mat ion of the superstructure due to subsidence<br />

in abutments/columns will affect carrying capacity . Calculations must be undertaken be<strong>for</strong>e<br />

deciding the degree of damage. In many instances differential subsidence has been taken into<br />

account during the design period and should there<strong>for</strong>e be included in the process of deciding the<br />

degree of damage.<br />

De<strong>for</strong>mation due to subsidence can also affect future maintenance costs since the long-term de<strong>for</strong>mation<br />

of concrete caused by creep will make jacking procedures more difficult.<br />

Carrying capacity will not be affected by subsidence of scaffolding.<br />

Both traffic safety, maintenance costs and the environment can be affected byabnormallong-tenn<br />

de<strong>for</strong>mation due to the bridge's fully laden weight.<br />

150 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9.2 CONCRETE ELEMENTS<br />

Conditions which trigger Maintenance<br />

When de<strong>for</strong>mation has lead to too Iowa carrying capacity measures must be taken immediately.<br />

Action should also be taken when de<strong>for</strong>mat ion spoils the appearance of a bridge.<br />

Procedures:<br />

* Jacking up and adjustment of the bearings (continuous span bridges)<br />

* Removal of unwanted loads such as asphalt<br />

* Strengthening or reconstruction<br />

* Replacement of elements<br />

Example 9.2-5<br />

Deflection ofa cantili vered slab due to insufficie nt<br />

rein<strong>for</strong>cement/incorrectly installed rein<strong>for</strong>cement.<br />

Type of Damage: 203<br />

De<strong>for</strong>mat ion of Concrete Elemen ts<br />

Degree of Damage &<br />

Consequences:<br />

3C<br />

Cause of Damage: 12<br />

Erroneous calculations<br />

Procedures:<br />

Strengthening within one year<br />

Example 9.2-6<br />

Bowing ora column caused by fonnwork left<br />

behind after completion,resulting in an increase of<br />

the ground pressure on the column.<br />

Type of Damage:<br />

203<br />

De<strong>for</strong>mation of Concrete Element<br />

Degree of Damage & Consequences: 3C<br />

Cause of Damage: 38<br />

Construction fault<br />

62<br />

Soil Pressure<br />

Procedures:<br />

Strengthening of the columns and replacement of<br />

materi als with lighter ones (E PS) within one year.<br />

<strong>Handbook</strong> <strong>for</strong> Bri dge <strong>Inspections</strong> 151


9.2 CONCRETE ELEMENTS<br />

Example 9.2-7<br />

De<strong>for</strong>mation caused by settlement of the scaffolding<br />

during the construction phase; this was subsequent<br />

ly levelled off with asphalt.<br />

Type of Damage: 203<br />

Defomlation of Concrete Element<br />

Degree of Damage &<br />

Consequences:<br />

I B<br />

Cause of Damage:<br />

31 Settl ement<br />

of scaffold ing<br />

Procedu res:<br />

None<br />

152 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


9.2 CONCRETE ELEMENTS<br />

204 Cracks in Concrete Elements<br />

Description<br />

Thi s category covers all hamlful cracks a nd fi ssures in concrete. Thus cracks in concrete which<br />

have been subject to stress from flexura l or tensile <strong>for</strong>ces are normal. However, these cracks must<br />

fall within certain limits.<br />

<strong>Bridge</strong>s containing pl ai n steel rein<strong>for</strong>cement bars can be subject to large cracks more widely spaced<br />

apart than is the case <strong>for</strong> ribbed rein<strong>for</strong>cement bars. Pre-stressed constructions do not nonnally suffer<br />

from cracking.<br />

Cause of Damage<br />

* Design fault - insufficient reinfo rcement! hi gh tension in the rein<strong>for</strong>cement during in-service<br />

condition.<br />

* Materials fault - an incorrect concrete mixture can produce shrinkage cracks. Aggregates which<br />

react to alkali can there<strong>for</strong>e react with alkali contained in cement and water and in the long tenn<br />

produce an expansion in the volume of the concrete. This can lead in turn to cracks.<br />

'" Construction fau lts - both an inadequate casting process and faulty finishing treatment may cause<br />

cracks during curing, cracks resulting from loss of plasticity, wastage due to dehydration or<br />

cracks caused by the heat of the curing process Itemperature gradients.<br />

'" Inadequate day-to-day maintenance - badly cleaned out joints may result in<br />

un<strong>for</strong>eseen loads.<br />

'" Environmental impact - hostile environment, e.g. cracks caused by chloride induced corrosion on<br />

rein<strong>for</strong>cement.<br />

'" Impacts from traffic, subsidence etc ..<br />

'" Accidental impacts - traffic collisions.<br />

'" In-service impacts - secondary damage.<br />

Possible Measurements<br />

'" Measuring the width and pattem of cracks<br />

'" Removal of concrete specimens, drilling out cores or thin sli cing.<br />

Degree of Damage/Consequences<br />

The degree of damage should be assessed in relation to the location of the cracks, extent, cause,<br />

probable development and the amount of stress the elements have been subjected to. In addition,<br />

climate impact may be of importance here.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 153


9.2 CONCRETE ELEMENTS<br />

Serious cracks and fi ssures can indicate too Iowa carrying capacity. They can also lead to corrosion<br />

of the rein<strong>for</strong>cement which also affects carrying capacity. Cracks or fi ssures pennitting the passage<br />

of dampness will be substantially more dangerous than dry cracks when taking corrosion Qfthe<br />

rein fo rcement into account.<br />

In most cases cracks and fi ssures wi ll be of consequence <strong>for</strong> maintenance costs and also <strong>for</strong> the<br />

environment dependent on their location.<br />

The followi ng rul e of thumb can be used to determine the degree of damage <strong>for</strong> cracks or fissures<br />

which could affect future maintenance costs:<br />

Sli ghtly Aggressive Environment (SAE): Crack/fissure < 0,5 mm 1M<br />

Crack/fissure 0,5· ],0 mm<br />

2M<br />

Crack/fissure > 1,0 mm<br />

3M<br />

Aggressive Environment CAE): Crack/fissure < 0,2 mm 1M<br />

Crack/fissure 0,2-0,5 mm<br />

2M<br />

Crack/fissure > 0,5 mm<br />

3M<br />

Cracks or fi ssures penetrated by dampness must always be assessed as irthey were located in an<br />

aggressive environment. Cracks or fissures in concrete situated in an aggressive environment<br />

should be checked fo r corrosion of the rein <strong>for</strong>cement by cutting away specimens in a few places.<br />

Conditions which Trigger Maintenance<br />

Very often cracks or fissures have been caused by other fonns o r damage such as de<strong>for</strong>mation,<br />

movement, lack of cleaning etc. Measures must be taken against primary damage be<strong>for</strong>e carrying<br />

out procedures fo r cracks and fissures. Similarly measures are required to be taken against cracks<br />

and fi sssures be<strong>for</strong>e other kinds of damage can develop, e.g. corrosion of the rein<strong>for</strong>cemellt, which<br />

can result in reduced carrying capacity and increased maintenance costs.<br />

Procedures<br />

Surface treatment, which provides permanent cover of the cracks/fi ssures.<br />

* Scaling of cracks/fissures<br />

* Injection of cracks/fi ssures<br />

* Strengthening<br />

~ FLEXURAL MOMENT<br />

JTOR510N<br />

"-~-I<br />

I<br />

/ //<br />

SHEARING<br />

!<br />

~L ______ -----1t<br />

CO"" "'""" COAD<br />

Fig1lre showillg diiferelll killlis of cracks!fi.HIIIY!S which call be caused by ex/ernalloalls<br />

154 <strong>Handbook</strong> f or <strong>Bridge</strong> <strong>Inspections</strong>


9.2 CONCRETE ELEMENTS<br />

Plastic Settlement Crack<br />

~~~?f ./<br />

T " A (<br />

If<br />

Crazing<br />

(ratk Caused by Reaction to Alkali<br />

Crack Caused by Thermal COlltraction<br />

(Heat During the Curing Process)<br />

Crack caused by ther al contraction<br />

eat un"g! ecurin9Process",,) ... ",~~<br />

Plastic Settlement Crack<br />

Crazing<br />

Plastic Settlement Crack<br />

Cracks Caused by Corrosion of the Rein<strong>for</strong>cement<br />

Figure showillg examples of differel1l types of c/'Gch 10 be/oulld ill COl/crete bridges.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 155


9.2 CONCRETE ELEMENTS<br />

Example 9.2-8<br />

Cracks on the deck of a suspension bridge caused<br />

by blocked joints. A total collapse is not anticipated.<br />

Refer to Chapter 9.8 <strong>for</strong> joints.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 3C<br />

Cause of Damage: 44<br />

Inadequate Maintenance<br />

Procedures:<br />

Chi selling out the concrete; casting ornew cross<br />

beams; installation of tight joints. To be carried oul<br />

within one year.<br />

Example 9.2-9<br />

Cracks under a bearing whi ch has been sited too<br />

near the edge.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 4C<br />

Cause of Damage: 13<br />

Poor Design Solutions<br />

Procedures:<br />

Reli eve pressure on the bearing immediately;<br />

strengthening the bearing shelfwithin a year.<br />

Example 9.2·10<br />

Cracks on a pier caused by a reaction to alkali. The<br />

cracks arc up to I mm wide and located in a aggres·<br />

sive environment.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 3M<br />

Cause of Damage: 25<br />

A Ikaline reactive Aggregates<br />

Procedures:<br />

Joints above the pi er should be sealed \ ... ·ithin 2<br />

years in order to reduce water leakages down on the<br />

pIer.<br />

156 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


Example 9.2-11<br />

9.2 CONCRETE ELEMENTS<br />

Cracks on a retaining wall caused by a reaction to<br />

alakali (con finned by structural analysis). De-icing<br />

salt on the pavement is normally not used. The<br />

width of the cracks does not exceed 0.8 mm. The<br />

site is not very accessible, and the public rarely go<br />

there.<br />

Type of damage:<br />

Cracks in Concrete Element<br />

Cause of Damage & Conseq uences:<br />

Cause of Damage:<br />

Alkaline reactive Aggregates<br />

204<br />

2M, IE<br />

25<br />

Procedures:<br />

Surface water should be drained orfand the bridge<br />

deck treated with waterproofing layer. This should<br />

be carri ed out within 5 years.<br />

Example 9.2-12<br />

Cracks in a concrete beam due to bowing. Statical<br />

calculations indicate that there is adequate rein<strong>for</strong>cement.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 2M<br />

Cause of Damage: 61<br />

Traffi c Loads<br />

Procedures:<br />

Treatment of the surface within 5 years with a coating<br />

of material designed <strong>for</strong> covering cracks.<br />

Example 9.2-13<br />

Crack in a wing wall due to subsidence.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 2M<br />

Cause of Damage: 82<br />

Consequenti al/Secondary Damage<br />

Procedures:<br />

Follow up by taking levell ing measurements. Once<br />

the subsidence has stopped the cracks can be injection<br />

filled.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 157


9.2 CONCRETE ELEMENTS<br />

Example 9.2-14<br />

Cracks in the side wa ll of an abutment due to skewed<br />

settlement. There is only minor traffic on the<br />

road. The settlement process has ceased.<br />

Type of damage: 204<br />

CracksIFissures of Concrete Element<br />

Cause of Damage & Consequences: 2.\1<br />

Cause of Damage: 82<br />

Consequential/Secondary Damage<br />

Procedure:<br />

Replace with lighter intil (E PS) together with injecti<br />

on of the cracks within 5 years.<br />

Example 9.2-15<br />

Cracks on lOp ofa pier caused by subsidence of the<br />

abutment. The settlement process has ceased, and<br />

the carrying capacity remains intact.<br />

Type of Damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 3.\1<br />

Cause of Damage: 82<br />

ConsequcntiallSecondmy Damage<br />

Procedures:<br />

Cracks to be sealed within one yea.<br />

Example 9.2-16<br />

Settlement crocks which occurred during the casting<br />

process.<br />

Type of Damage: 204<br />

Crocks inConcrete Element<br />

Cause of Damage & Consequences: 3.\1<br />

Cause of Damage: 38<br />

Construction Fault<br />

Procedures:<br />

Seal the crocks within one year.<br />

158 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


Example 9.2-17<br />

9.2 CONCRETE ELEMENTS<br />

Through cracks in a newly cast bridge deck caused<br />

by the curing temperature when casti ng on to cold<br />

concrete.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences: 3M<br />

Cause of Damage: 35<br />

Inadequate curing Procedures<br />

Procedures:<br />

Cracks to be injection filled within onc year.<br />

Example 9.2-18<br />

Dampness and lime precipita tion in a crack on the<br />

underneath orthe deck of a prefabricated footbridge.<br />

None of the cracks exceed 0.7 mm in width.<br />

Type of damage: 204<br />

Cracks in Concrete Element<br />

207<br />

Leakage/Dampness of Concrete<br />

Cause of Damage & Consequences: 3M<br />

Cause of Damage: 67<br />

Shrinkage/creeping<br />

Procedures:<br />

Cracks to be sealed within 2 years.<br />

Example 9.2-19<br />

Lime precipitation in shrinkage cracks in a culvert<br />

due to earlier water penetration which has now<br />

dried out after the lime products closed the cracks;<br />

the leakage then stopped. There is a lot of pedestrian<br />

traffic through this culvert.<br />

Type of damage:<br />

Cracks in Concrete Element<br />

Cause of Damage & Consequences:<br />

Cause of Damage:<br />

Shrinkage/creeping<br />

204<br />

(M,3E<br />

67<br />

Procedures:<br />

The surface of the concrete should be sandblasted<br />

within one year in order to improve its appearance.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 159


9.2 CONCRETE ELEMENTS<br />

205 Ruptures of Concrete Element<br />

Description<br />

Extensive damage to the whole or part of a bridge element, c.g. cracks or areas of broken orf concretc.<br />

Cause of Damage<br />

* Design fault - attention has not been paid to concentrated loads; there is little room <strong>for</strong><br />

expanSion.<br />

* Construction fau lt - post-tensioning be<strong>for</strong>e the concrete had achieved its prescribed fi rmness can<br />

lead to rupture.<br />

* Insufficient day-to day maintenance.<br />

* Impacts from traffic, ground pressure and the li ke.<br />

* Accidents - e.g. traffic impacts.<br />

* In-service damage - e.g. secondary damage.<br />

Degree of Damage/ Conseq uences<br />

The degree of damage should be assessed based on its location, size and probable development. A<br />

high degree of damage shou ld be allocated to load bearing elements.<br />

For load bearing elements, ruptures will affect the carrying capacity. Regarding non-load bearing<br />

elements, a rupture may affect traffic safety, future maintenance costs and/or the environment.<br />

Conditions which trigger Maintenance<br />

Immediate acti on must be taken if the bridge's canying capacity is to low or traffic safety has been<br />

reduced.<br />

If the damage has affected maintenance costs, acti on should be taken be<strong>for</strong>e other damage leading<br />

to increased maintenance costs develops.<br />

Procedures<br />

* Mechanical repairs<br />

* Replacement<br />

* Strengthening.<br />

160 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


Example 9.2-20<br />

9.2 CONCRETE ELEMENTS<br />

Broken cross-beam Of sllspcnsion bridge resulting<br />

from blockedjoint .<br />

Type of Damage: 205<br />

Ruptures of Concrete El ement<br />

Degree of Damage ICon sequences: 3C<br />

Cause of Damage: 82<br />

Consequential/Secondary Damage<br />

Procedures:<br />

Existing cross-beam to be CUi away and replaced<br />

within onc year.<br />

Exam ple 9.2-21<br />

Broken beam res ulting from a traffic accident.<br />

Reduced carrying capaci ty as well as the ri sk of<br />

pieces of concrete fall ing off.<br />

Type of Damage: 205<br />

Ruptures of Concrete El ement<br />

Degree of Damage & Consequences: 4C, 4T<br />

Cause of Damage: 71<br />

Vehicular Impaci Damage<br />

Procedures:<br />

<strong>Bridge</strong> to be closed to traffi c until repairs effected.<br />

Example 9.2-22<br />

Broken ba llast wall due to movement in an abut ­<br />

ment caused by ground prcssurc.<br />

Type of Damage: 205<br />

Rupture of Concrete Element<br />

Degree of Damage & Consequences: 2M<br />

Causc ofDamagc: 62<br />

Soi I Pressure<br />

82<br />

Consequential/Secondary Damage<br />

Pr ocedures:<br />

Replace with lighter in fi ll materials (EPS) and<br />

effect repairs to the ballast wall within 5 years.<br />

<strong>Handbook</strong> <strong>for</strong> Bri dge Inspect ions 161


9.2 CONCRETE ELEMENTS<br />

206 Damage to Concrete Surface<br />

Treatment<br />

Descri ption<br />

Damage to the surface treatment of concrete bridge elements, i.c. water repellent impregnation,<br />

painting/coating, whitewashing/pore filling. Flaking, cracking, bli stering, and discoloration can be<br />

incl uded here; additionally, the surface treatment might not fu lftl lhe required in-service standards.<br />

Surface treatment applied to concrete must be able to protect the concrete from environmental<br />

impacts and improve its general appearance.<br />

Cause of Damage<br />

• Design Fault - incorrect type of surface treatment chosen.<br />

• Material Fault - incorrect type of surface treatment applied.<br />

• Construction Fault - poor pre-treatment of the surface, or the material was appl ied during damp<br />

or cold weather.<br />

• Insufficient operation/maintenance of the surface treatment.<br />

• Environmental impacts - a hosti le environment can break down the surface treatment faster than<br />

expected<br />

• In-service damage - regul ar wear and tear.<br />

Possible Materials Testing<br />

• Thickness of the surface treatment<br />

• Adhesion between the surface layer and concrete.<br />

• Impregnation depth to concrete of repellent impregnation.<br />

• Measuring chloride content and depth of carbonisation.<br />

Degree of Damage/Consequences<br />

All types of surface treatment gradually become broken down by the environmental influence. The<br />

degree of damage a ll ocated shall reflect the time remaining be<strong>for</strong>e the surface treatment requires<br />

renewal, i.e. be<strong>for</strong>e it loses its protective properties. Damage to the surface treatment wi ll affect<br />

maintenance costs and result in increased chl oride penetration and speed of development of carbonisation.<br />

These last two items can, in addition, lead to corrosion of the rein<strong>for</strong>cement and to spalling.<br />

162 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong>


9.2 CONCRETE ELEMENTS<br />

If the damage is extensive and/or the surface treatment has lost its protective qualities, a new layer<br />

of surface treatment must be appl ied. When the damage is minor, action need only be taken be<strong>for</strong>e<br />

any other types of damage develope and be<strong>for</strong>e the damage becomes so extensive that the enticre<br />

surface treatment has to be renewed.<br />

Conditions which trigger Maintenance<br />

Procedures:<br />

. Regular cleaning and renewal orthe surface treatment<br />

. Removal orthe existing treatment and the application ora new coating.<br />

Example 9.2-23<br />

Localised spall ing of the surface treatment ofa<br />

concrete parapet.<br />

Type of Damage: 206<br />

Damage to the Concrete Surface Treatment<br />

Degree of Damagei<br />

Consequences:<br />

Cause of Damage:<br />

Construction Fault<br />

3M, 2E<br />

38<br />

Procedures:<br />

Maintenance measures to be taken within three<br />

years <strong>for</strong> damaged surface treatment.<br />

Example 9.2-24<br />

Surface treatment damaged by wind and weather.<br />

This bridge has been greatl y subjected to chl oride<br />

attack, and the surface treatment has no longer any<br />

of its protective qualit ies. The appearance o f the<br />

bridge can hardly be described as attmctive.<br />

Type of Damage: 206<br />

Damage to the Concrete Surface Treatment<br />

Degree of Damage/<br />

Consequences:<br />

Cause of Damage:<br />

Inadequate Maintenance<br />

Normal Wear and Tear<br />

3M, 3E<br />

44<br />

81<br />

Procedures:<br />

The ent ire surface treatment should be removed and<br />

renewed within three years.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> <strong>Inspections</strong> 163


9.2 CONCRETE ELEMENTS<br />

207 LeakagesJ1)ampness of<br />

Concrete<br />

Description<br />

This covers water seeping through cracks, leakage between prefabricated concrete elements and/or<br />

dampness attack resulting fro m leaks or fa iled attention to detai ls. Leakages Idampncss attacks can<br />

produce corrosion orthe rein<strong>for</strong>cement and spall ing to the covering. Leakage leads to discoloration<br />

of the concrete (lime deposits on the surface).<br />

Cause of Damage<br />

* Design Fault - unsuccessful design causing leakage/dampness ..<br />

* Material Fault - incorrect composition of the concrete can lead to porosity so that the concrete is<br />

not water resistant.<br />

* Construction Fault - concrete has nol been correctly vibrated which has resulted in porosity.<br />

* Depressions cause insufficient drainage of water and the risk ofleakage and dampness attacks.<br />

* Insufficient day· to-day operation/or maintenance.<br />

* In-service damage, e.g. secondary damage.<br />

Degree of Damage/Consequences<br />

The degree of damage should be selected depending on the age of the bridge, the extent of the lea·<br />

kage/dampness impact and the speed at which other damage can develop.<br />

Leakage/dampness impact can affect maintenance costs and/or traffic safety in so far as icicles and<br />

icy road surfaces can <strong>for</strong>m in winter.<br />

Conditions which Trigger Maintenance Measures<br />

Measures should be taken to stop leakage/dampness impact be<strong>for</strong>e the risk arises of other damage<br />

develop ing such as corrosion oflhe re in<strong>for</strong>cement and spalling. If, fo r example, reduced traffic<br />

safety or icy sections can result from leakage/dampness impact, then immediate action must be<br />

taken.<br />

Procedures<br />

* Sealing, injection fill ing<br />

* Alteration to the water drainage system<br />

* Mechanical repairs to the concrete<br />

* Installation of new waterproofing layer on the bridge deck.<br />

164 <strong>Handbook</strong> <strong>for</strong> Bri dge Inspect ions


Example 9.2-25<br />

9.2 CONCRETE ELEMENTS<br />

Leakage through joints between concrete elements<br />

because ofinadequalc seal ing ca using a dampness<br />

attack on the underside orthe bridge.<br />

The elements are prestressed and there<strong>for</strong>e particularly<br />

vulnerable to corrosion of the rein<strong>for</strong>cement.<br />

The bridge deck has been exposed to de-icing salt.<br />

Type of Damage: 207<br />

LeakagelDampness of Concrete<br />

Degree of Damage &<br />

Consequences:<br />

3M<br />

Cause of Damage: 38<br />

Construction Fault<br />

Procedures:<br />

In sta llation ornew waterproofing layer on the bridge<br />

deck within one year<br />

Example 9.2-26<br />

Leakage through joints between the clements of a<br />

pedestrian culvert because of inadequate seal ing.<br />

Type of Damage:<br />

Lcakage/Dampncss of Concrete<br />

Degree of Damage &<br />

Conseq uences:<br />

Cause of Damage:<br />

Construction Fault<br />

207<br />

3T, 2M<br />

38<br />

Procedures:<br />

The joints should be sealed within three years.<br />

Example 9.2-27<br />

Serious leakage in the region of a power cable duct.<br />

There is a pathway under the bridge.<br />

Type of Damage: 207<br />

Leakage/Dampness of Concrete<br />

208<br />

Di scoloration of Concrete Element<br />

Degree of Damage ICon sequences: 2M, 2E<br />

Cause of Damage : 38<br />

Construction Fault<br />

Procedures:<br />

Leakage to be sealed within five years.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 165


9.2 CONCRETE ELEMENTS<br />

Example 9.2-28<br />

Leakage through the bridge deck over a small ,<br />

badl y cast area. The bridge is approx imately 30<br />

years old and has not been salted.<br />

Type of Damage: 207<br />

Leakage/Dampness of Concrete<br />

211<br />

Honeycombing<br />

Degree ofDamagc/Consequcnces: 2M<br />

Cause of Damage: 38<br />

Construction Fault<br />

Procedures:<br />

Installation of new waterproofing layer and wearing<br />

course within five years<br />

Example 9.2-29<br />

Dampness and li me deposits on the underside of the<br />

bridge deck indicate the existence of<br />

leakages/dampness impact <strong>for</strong> some time. Both the<br />

wearing surface and the membrane are worn<br />

through.<br />

Type of Damage: 207<br />

Leakage/Dampness of Concrete<br />

Degree ofDamagc/Conscqucnces: 2M<br />

Cause of Damage: 82<br />

Conseq uentiaVSccondary Damage<br />

Procedures:<br />

Installation of new waterproofing layer and wea~<br />

ring course within five years.<br />

Example 9.2-30<br />

Leakage between cross ~ beams has been caused by<br />

porous concrete and leaky joints directly above the<br />

c ross~beams. The water has worn away the surface<br />

treatment of the steel.<br />

Type of Damage: 207<br />

Leakage/dampness of Concrete Element<br />

Degree of Da mage & Consequences: 3M<br />

Cause of Damage:<br />

II<br />

Incorrect Choice of Materials 38<br />

Construction Fault<br />

Procedures:<br />

No action is required <strong>for</strong> the concrete cross~beams.<br />

The joints, however, must be cleaned out and sealed<br />

within three years. In addition, the steel elements<br />

should be painted.<br />

166 <strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions


9.2 CONCRETE ELEMENTS<br />

Example 9.2-31<br />

Leakage through the bridge deck made of very<br />

poor, porous concrete has resulted in severe corrosion<br />

orthe re in fo rcement, spalling and crumbling<br />

concrete.<br />

Type of Damage: 207<br />

Leakage/Dampness of Concrete<br />

209<br />

Insufficien t/damaged covering<br />

210<br />

213<br />

Spalling of Concrete Element<br />

214<br />

Corrosion of the Rein<strong>for</strong>cement<br />

Degree of Damage/Consequences: 3C<br />

Cause of Damage: 38<br />

Construction Fault<br />

Procedures:<br />

Rebui lding ofhridge deck within I year.<br />

Example 9.2-32<br />

Leakage through the cast-joints of a retaining wall<br />

leads to weathering orthe concrete. The retaining<br />

wall is located adjacent and parallell to the road.<br />

Type of Damage: 207<br />

Leakage/Dampness of Concrete<br />

208<br />

Di scoloration of Concrete Element<br />

210<br />

Weathering of Concrete<br />

Degree of Damage/Consequences: 1 C, 2M, 3E<br />

Cause of Damage: 38<br />

Construction Fault<br />

Procedures:<br />

Inj ection filling of the cast joints, and cleaning<br />

up/treatment of the surface material within three<br />

years.<br />

<strong>Handbook</strong> <strong>for</strong> <strong>Bridge</strong> Inspect ions 167

Hooray! Your file is uploaded and ready to be published.

Saved successfully!

Ooh no, something went wrong!