1. B. DATA ON CSEB<br />
TECHNICAL SPECIFICATIONS (5% CEMENT STABILISED BLOCKS)<br />
Dry compressive crushing strength σc (At 28 : 5 to 7 Mpa<br />
days)<br />
Wet compressive crushing strength σc (At 28 : 3 to 4 Mpa (after 24 h. immersion)<br />
days)<br />
Dry bending crushing strength σb (At 28 days) : 0.5 to 1 Mpa<br />
Dry shear crushing strength (At 28 days) : 0.4 to 0.6 Mpa<br />
Water absorption by weight (At 28 days) : 8 to 10 % (after 24 h. immersion)<br />
Apparent bulk density (dry) : 1,900 to 2,000 kg/m 3<br />
Coefficient of conductivity : 0.81 to 0.93 W/m°C<br />
Time lag : 10 – 12 hours for 40 cm thick<br />
Embodied energy per m 3 of finished masonry : 1,112.36MJ / m 3<br />
(This value has to be compared with country fired bricks = 4,501.25 MJ / m 3<br />
Carbon emission (CO2) per m3 of finished : 100.11 Kg / m<br />
masonry<br />
3<br />
(This value has to be compared with country fired bricks = 441.12 Kg / m3 Notes:<br />
� Compressive strength values are for <strong>Auroville</strong> soil<br />
(red sandy soil of lateritic origin with iron oxide), compressed with the Auram press 3000<br />
� These mechanical characteristics are influenced by:<br />
- The soil quality, the compression ratio and the force applied by the press<br />
- The quality of manufacturing and especially curing<br />
- The quality and percentage of stabilizer<br />