<strong>BP</strong>TO 2380 Typical Inspections vs. MIL-PRF-23699F-STD Specification<br />
The values shown here are representative of current production. Some are controlled by manufacturing specifications,<br />
while others are not. All of them may vary within modest ranges.<br />
FED. TEST<br />
ASTM or SAE METHOD<br />
MILITARY SPECIFICATION TESTS <strong>BP</strong>TO MIL-PRF-23699F STANDARD STD. NO. 791<br />
2380 MIN. MAX.<br />
Viscosity, cSt @ <strong>–</strong> 40°C (<strong>–</strong> 40°F) . . . . . . . . . . . . . . . . . . . . 7950 — 13,000 D2532<br />
% change <strong>–</strong> 40°C (<strong>–</strong> 40°F), 72 hrs . . . . . . . . . . . . . . . . . 0.7 — ±6 D2532<br />
cSt @ 100°C (212°F). . . . . . . . . . . . . . . . . . . . . . . . . . . . . 4.97 4.90 5.40 D445<br />
cSt @ 40°C (104°F). . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 24.2 23.0 — D445<br />
Flash point, °C . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 265 246 — D92<br />
Pour point, °C . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . <strong>–</strong> 57 — <strong>–</strong> 54 D97<br />
TAN, mgKOH/g . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0.43 — 1.00 SAE-ARP5088<br />
Evaporation loss, %, 6.5 hrs. @ 204°C (400°F) . . . . . . . . 3.0 — 10 D972*<br />
Foam 1 24°C (75°F), ml/collapse time . . . . . . . . . . . . . . . 9/0 — 25/0 D892*<br />
Foam 2 93.5°C (200°F), ml/collapse time . . . . . . . . . . . . 8/0 — 25/0<br />
Foam 3 24°C (75°F), ml/collapse time . . . . . . . . . . . . . . . 8/0 — 25/0<br />
Rubber compatibility ..................................................... 3604/3433<br />
AMS No. 3217/1, % Swell, 72 hr. @ 70°C (158°F) . .. 14.4 5 25<br />
AMS No. 3217/4, % Swell, 72 hr. @ 204°C (400°F). . 9.9 5 25<br />
Si Rubber, % Swell, 96 hr. & 121°C (250°F) . . . . . . . . 11.4 5 25<br />
Tensile strength loss, %. . . . . . . . . . . . . . . . . . . . . . . . <strong>–</strong> 7.3 — 30<br />
Compatibility. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Pass Pass 3403*<br />
Turbidity . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . Pass None<br />
Sediment, mg/l . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 3.0 20<br />
Storage stability, 6 wks.. . . . . . . . . . . . . . . . . . . . . . . . . . . . . Pass Pass Part 4.4.2 of 23699 Spec.<br />
Thermal stability and corrosivity, 274°C (525°F) ........... 3411<br />
% Vis change. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0.6 — 5.0<br />
TAN change, mg KOH/g . . . . . . . . . . . . . . . . . . . . . . . . . . 2.2 — 6.0<br />
Metal wt. change, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . <strong>–</strong> 0.2 — 4.0<br />
Sediment 1.2 micron, mg/l . . . . . . . . . . . . . . . . . . . . . . . . . . 0.9 — 10 3010<br />
Ash, mg/l. . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0.1 — 1<br />
Corrosion and oxidative stability, 72 hrs. @ 175°C (347°F) 5308*<br />
Steel, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +0.02 — ±0.2<br />
Ag, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0 — ±0.2<br />
Al, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.02 — ±0.2<br />
Mg, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.02 — ±0.2<br />
Cu, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.07 — ±0.4<br />
Vis, change @ 37.8°C (100°F), % . . . . . . . . . . . . . . . . . . 8.0 — <strong>–</strong> 5 to +15<br />
TAN change, mgKOH/g. . . . . . . . . . . . . . . . . . . . . . . . . . . 0.11 — 2.0<br />
Sludge, mg/100ml . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 1.1 — 50<br />
Corrosion and oxidative stability, 72 hrs. @ 204°C (400°F) 5308*<br />
Steel, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.01 — ±0.2<br />
Ag, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0 — ±0.2<br />
Al, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.01 — ±0.2<br />
Mg, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 0 — ±0.2<br />
Cu, mg/cm 2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . +.04 — ±0.4<br />
Vis, change @ 37.8°C (100°F), % . . . . . . . . . . . . . . . . . . 18.9 — <strong>–</strong> 5 to +25<br />
TAN change, mgKOH/g. . . . . . . . . . . . . . . . . . . . . . . . . . . 1.1 — ±3.0<br />
Sludge, mg/100ml . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 1.4 — 50<br />