70<br />

6O<br />

E<br />

z 50<br />

~E<br />

Ul<br />

I/1<br />

E<br />

30<br />

C<br />

"~ 20<br />

fll<br />

e-<br />

10<br />

0<br />

- Z<br />

IN<br />

120<br />

I/1<br />

I/1<br />

-~80-<br />

m<br />

I/1<br />

O!<br />

t--<br />

5-.<br />

.JO<br />

60 -<br />

I/1<br />

E ~0 -<br />

o ~<br />

c-<br />

¢::<br />

~,20-<br />

- 0<br />

103<br />

Unbushed achieved<br />

\<br />

Bushed predicted performance from local stress measurements<br />

performance ~ , ~ . ~ - achieved per formance<br />

I I I J<br />

104 105 106 10 ?<br />

Log mean endurance (cycles)<br />

Fig 36 Estimation <strong>of</strong> endurance <strong>of</strong> bushed lugs using local stress<br />

history measurements. Mean stress = 153(95) MN/m2<br />