TYPE HEAT TREATMENT<br />

4320 NORMALIZED 1700° F. — AUSTENITIZED 1700° F.<br />

CHEMICAL ANALYSIS C Mn P S Si Cr Ni Mo Cu Al V W B<br />

.18 .61 .010 .014 .29 .50 1.79 .23 .09 .021 — — —<br />

ROUND SECTION WITH SAME HARDNESS AT MID-RADIUS<br />

OIL QUENCH<br />

.4-.5 Hv 1" 2" 3" 4" 5" 6" ~9"<br />

MILD WATER<br />

AIR<br />

QUENCH<br />

1" 2" 3" 4" 5" 6" 7" QUENCH 1" 2" 3" 4" 5" 6" 10" 15"<br />

55° F /S 25° F /S 12° F /S 7° F /S 290° F /M 200° F /M 80° F /M 32° F /M 27° F /M 19° F /M 13° F /M 12° F /M 9° F /M 6° F /M<br />

COOLING<br />

RATE<br />

LEGEND<br />

AS COOLED<br />

1000˚ F. TEMPER-2 HOURS<br />

SAE HARDENABILITY BAND<br />

AUSTENITIZING TEMPERATURE<br />

1700˚ F.<br />

60<br />

614<br />

50<br />

484<br />

74<br />

40<br />

372<br />

30<br />

ROCKWELL<br />

“C” HARDNESS<br />

283<br />

20<br />

230<br />

90<br />

185<br />

80<br />

150<br />

70<br />

128<br />

BRINELL HARDNESS – 3000 KG.<br />

60<br />

ROCKWELL<br />

“B” HARDNESS<br />

107<br />

10 15 20 27 11 /2" 11 3 1 5 48<br />

4" /4" /4" 2 /2" 6"<br />

INTERFACE<br />

SIXTEENTHS FROM QUENCHED END OF JOMINY BAR AIR HARDENABILITY DISTANCE