BINDER PITCH QI CONTENT – ALUMINIUM ANODE<br />

The <strong>effect</strong> <strong>of</strong> conditions in <strong>the</strong> “tunnel head” on <strong>the</strong> amount <strong>of</strong><br />

normal QI formed is shown in Figure 7.<br />

16<br />

14<br />

12<br />

10<br />

Effect <strong>of</strong> Tunnel-Head Temperature<br />

on Tar QI Content<br />

8<br />

6<br />

8.0<br />

7.5<br />

7.0<br />

6.5<br />

6.0<br />

5.5<br />

870 900 925 955 980 1010 1035<br />

Tunnel-Head Temp., °C<br />

Effect <strong>of</strong> Coal Bulk Density<br />

on Tar QI<br />

640 655 670 690 705 720 735 750<br />

Bulk Density (Dry, Cone) Kg/m 3<br />

Figure 7 – Tunnel Head Effect on QI Formation<br />

As Figure 7 indicates, <strong>the</strong>re are two major factors which affect <strong>the</strong><br />

amount <strong>of</strong> normal QI which is formed in <strong>the</strong> coke oven. These<br />

factors are <strong>the</strong> temperature in <strong>the</strong> “tunnel head” and <strong>the</strong> bulk density<br />

<strong>of</strong> <strong>the</strong> coal packed in <strong>the</strong> coke oven. The affect <strong>of</strong> temperature is<br />

easy to explain, but <strong>the</strong> affect <strong>of</strong> <strong>the</strong> bulk density <strong>of</strong> <strong>the</strong> coal is not as<br />