GARTEUR LIMITED<br />

Test fluids<br />

Coating<br />

post plating<br />

treatment<br />

Ethylene<br />

Glycol<br />

Turco 5948 Jet A1 Skydrol<br />

ED Zinc - Ni none p general attack<br />

(-93mg)<br />

passivated p edge attack<br />

(-125mg)<br />

p<br />

p<br />

p<br />

p<br />

ED Zn-Co-Fe none p edge attack<br />

(-61mg)<br />

passivated p slight edge attack<br />

(-15 mg)<br />

p<br />

p<br />

discolouration<br />

(-19mg)<br />

p<br />

(+30 mg)<br />

ED <strong>Cadmium</strong> none p<br />

(-11mg)<br />

general attack<br />

(-140mg)<br />

passivated p general attack<br />

(-334mg)<br />

p<br />

p<br />

discolouration<br />

(-22mg)<br />

p<br />

(-68mg)<br />

SermeTel none p p p p<br />

topcoat p p p p<br />

Delta-tone<br />

p<br />

(+18mg)<br />

p<br />

(+166mg)<br />

p<br />

p<br />

(+14mg)<br />

ED Aluminium p p p p<br />

IVD Aluminium none p<br />

(+23mg)<br />

passivated p<br />

(+17mg)<br />

slight edge attack<br />

(+19mg)<br />

slight edge attack<br />

(+15mg)<br />

p - no visual damage<br />

Table G3; Coating performance determined using Shorts total immersion tests<br />

GARTEUR SM/AG17 TP128 Page 91