GARTEUR LIMITED<br />

1 Dry grit blast with fine alumina 180-220 mesh<br />

2 Anodically cleaned<br />

3 Electroplating in Zincrolyte NCZ CF<br />

Voltage ~2.8V<br />

Current density ~2.5A/dm 2<br />

Plating time 35 minutes<br />

4 Passivation in Udyfin 7748<br />

Concentration 30ml/litre<br />

pH 1.6<br />

Immersion time 35-40 seconds<br />

Table A3; Zinc-cobalt-iron electroplating schedule<br />

Chemical<br />

Concentration<br />

(gm/litre)<br />

Ammonium chloride 171.5<br />

Nickel chloride 73.8<br />

Zinc chloride 16.7<br />

Boric acid 20.3<br />

BOE-NIZ LHE 30.3<br />

Table A4; Composition of CorroBan ® zinc-nickel<br />

electroplating bath<br />