GARTEUR LIMITED<br />

Coating Passivated Mean Ig<br />

(µA.cm- 2 )<br />

R a<br />

(mdd)<br />

R g<br />

(mdd)<br />

ED cadmium no 4.2 10.0 4.1<br />

yes 4.8 6.7 0.8<br />

ED zinc-nickel no 4.7 4.2 -1.7<br />

yes 9.2 1.2 -4.7<br />

ED zinc-cobalt-iron no 4.5 19.9 14.0<br />

yes 6.4 14.3 8.4<br />

PVD aluminium no 9.7 12.2 6.3<br />

yes 8.5 6.5 0.6<br />

ED aluminium no 9.5 9.1 3.2<br />

yes 9.1 4.4 -1.5<br />

UMS aluminium -<br />

magnesium<br />

no 6.1 14.2 8.3<br />

yes 4.9 9.9 4.0<br />

SermeTel 984 4.0 11.7 5.8<br />

984/985 4.7 6.7 0.8<br />

Delta-tone 9.6 16.5 10.6<br />

Table D3; Average galvanic current densities, R a and R g parameters for galvanic<br />

couples for 2014-T6 aluminium alloy in contact with metal coatings<br />

Coating Passivated Mean Ig<br />

(µA.cm- 2 )<br />

R a<br />

(mdd)<br />

R g<br />

(mdd)<br />

ED cadmium no 4.4 7.1 2.9<br />

yes 4.2 6.2 2.0<br />

ED zinc-nickel no 5.0 3.3 -0.9<br />

yes 9.0 2.2 -2.0<br />

ED zinc-cobalt-iron no 5.1 14.4 10.2<br />

yes 7.6 10.6 6.4<br />

PVD aluminium no 8.6 12.0 7.8<br />

yes 7.0 10.4 6.2<br />

ED aluminium no 7.4 6.2 2.0<br />

yes 8.0 3.2 -1.0<br />

UMS aluminium -<br />

magnesium<br />

no 4.9 12.9 8.7<br />

yes 5.3 8.1 3.9<br />

SermeTel 984 4.1 9.3 5.1<br />

984/985 4.6 8.7 4.5<br />

Delta-tone 5.7 13.2 9.0<br />

Table D4; Average galvanic current densities, R a and R g parameters for galvanic<br />

couples for 7075-T6 aluminium alloy in contact with metal coatings<br />