REWARI KANPUR PIPELINE<br />

PROJECT<br />

HIGH FREQUENCY ELECTRIC WELDED<br />

(HFW) LINE PIPE<br />

DOCUMENT NUMBER<br />

0068-00-SPC-2002<br />

Revision 0<br />

TYPE OF INSPECTION<br />

Wall thickness measurement<br />

FREQUENCY OF INSPECTION<br />

The wall thickness of each pipe shall be checked along the<br />

circumference at both ends and at the mid location of pipe<br />

body at 12 o'clock, 3 o'clock, 6 o'clock and 9 o'clock<br />

positions<br />

Wall thickness shall be measured and recorded at least 3<br />

times per operating shift (12 hours maximum).<br />

10.2.3 SAMPLES AND TEST PIECES FOR MECHANICAL TESTS<br />

10.2.3.2 TEST PIECES FOR THE TENSILE TEST<br />

Longitudinal tensile tests shall be carried out on a strip specimen. The strip specimen<br />

shall be tested without flattening.<br />

The transverse tensile tests shall be carried out on flattened rectangular specimen.<br />

For weld tensile test: Inside and outside flash of weld in excess of pipe wall thickness<br />

shall be removed from the specimen either by grinding or machining. Specimen shall be<br />

tested for ultimate tensile strength only.<br />

10.2.3.3 TEST PIECES FOR THE CVN IMPACT TEST<br />

In addition to the specimen taken from the body of the pipe, three transverse<br />

specimens with weld in middle and three transverse specimens with Heat Affected<br />

Zone (HAZ) in the middle shall also be taken. When either full size or sub-size<br />

transverse specimen as per API Spec 5L, Table 14 is not possible to obtain,<br />

transverse specimen of either <br />

may be obtained.<br />

When such sub-size specimens are used, the acceptance of the<br />

individual/average absorbed energy values shall be established as per API Spec<br />

5L Para 9.8.1 and as modified in this specification.<br />

10.2.3.4 TEST PIECES FOR DWT TEST<br />

Two transverse specimens shall be taken from one length of pipe per heat per lot<br />

of 100 pipes per <strong>com</strong>bination of pipe size and specified wall thickness. Unless<br />

specified otherwise, the test shall be conducted at +32F (0C).<br />

10.2.4 TEST METHODS<br />

10.2.4.3 CVN IMPACT TEST<br />

The charpy test shall be carried out in accordance with ASTM A 370.<br />