Prophecy Platinum Corporation – <strong>Wellgreen</strong> Property – <strong>Project</strong> 50149-001<br />

and nickel recoveries and enhance concentrate grade in the bulk concentrate, the effect of talc pre-<br />

flotation and CMC as silicate depressant were examined. In one test talc was floated ahead of the bulk<br />

copper and nickel flotation with frother. The results are shown in Figure 20.<br />

Recovery, %<br />

Recovery, %<br />

100<br />

80<br />

60<br />

40<br />

20<br />

Rougher Kinetics, Cu<br />

0<br />

0 2 4 6 8 10 12 14 16 18 20 22<br />

100<br />

80<br />

60<br />

40<br />

20<br />

Time, min<br />

Rougher Kinetics, Pt<br />

0<br />

0 2 4 6 8 10 12 14 16 18 20 22<br />

It can be concluded that:<br />

Time, min<br />

Recovery, %<br />

100<br />

80<br />

60<br />

40<br />

20<br />

Talc Pre-float<br />

CMC<br />

No CMC<br />

Talc Pre-float<br />

CMC<br />

No CMC<br />

Recovery, %<br />

Recovery, %<br />

100<br />

80<br />

60<br />

40<br />

20<br />

SGS Minerals Services<br />

Rougher Kinetics, Ni<br />

0<br />

0 2 4 6 8 10 12 14 16 18 20 22<br />

100<br />

80<br />

60<br />

40<br />

20<br />

Rougher Kinetics, Au<br />

0<br />

0 2 4 6 8 10 12 14 16 18 20 22<br />

Time, min<br />

Time, min<br />

Rougher Kinetics, Pd<br />

0<br />

0 2 4 6 8 10 12 14 16 18 20 22<br />

Talc Pre-float<br />

CMC<br />

No CMC<br />

Time, min<br />

Figure 20: Effect of Talc Pre-flotation and CMC on Rougher Flotation<br />

Talc pre-float<br />

CMC<br />

No CMC<br />

Talc Pre-float<br />

• Effect of CMC: CMC was applied to depress silicates. It was stage added to the first three<br />

rougher stages at 60 g/t. CMC had minimal overall impact on Cu, Ni and PGM recoveries. The<br />

slight increase in Au recovery is likely due to inherent process variation.<br />

• Effect of talc pre-float: Before collection of a first rougher concentrate, talc was floated using the<br />

addition of frother. It can be clearly observed in Table 8 that there was significant loss of Cu, Ni<br />

and PGM in the talc pre-float concentrate.<br />

CMC<br />

No CMC<br />

28